MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Total Finathene® 6002 HDPE, blow molding, pipe  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Blow Molding Grade

Material Notes: FINATHENE® 6002 is a high density polyethylene produced by the slurry loop low pressure polymerization process.

FINATHENE® 6002 has been especially developed for the manufacturing of toys and of blow molded bottles for diverse non-aggressive liquids such as food, oil and cosmetics. Its low melt viscosity is particularly suitable for high output processing equipment. Its high rigidity is especially appreciated when bottle weight reduction is critical.

FINATHENE® 6002 is best processed at temperatures between 180 and 220°C.

Information provided provided by Total Petrochemicals.

Total Petrochemicals includes former Fina and Atofina plastics product lines.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.959 g/ccISO 1183
Environmental Stress Crack Resistance 15 hourASTM D1693-70
Melt Flow 0.30 g/10 min
@Load 2.16 kg
ISO 1133
 1.4 g/10 min
@Load 5.00 kg
ASTM D 1238
High Load Melt Index 28 g/10 min
@Load 21.6 kg
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 26.0 MPaISO 527
Tensile Strength, Yield 28.0 MPaISO 527
Elongation at Break >= 700 %ISO 527
Elongation at Yield 8.0 %ISO 527
Flexural Modulus 1.50 GPaISO 178
Tensile Impact Strength 80.0 kJ/m²Notched, -30°C; ISO 8256
 230 kJ/m²Notched, 23°C; ISO 8256
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 128 °CISO 306
 
Descriptive Properties
Food ApprovalThis material complies with the main regulations concerning non-toxicity of plastics materials in contact with food stuffs.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chevron Phillips HiD® 99416 with Food Grade Antistat HDPE Blow Molding Resin
Celanese 7110 LDPE polymer for medical
Braskem HB0454HR HDPE Blow Molding Polyethylene Copolymer
LyondellBasell Alathon® L5040 High Density Polyethylene, Blow Molding/Extrusion Grade
LyondellBasell Petrothene® GA818073 Linear Low Density Polyethylene

PFINAP064 / 38647

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.