MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
SABIC ULTEM™ Resin CRS5011R Polyetherimide (PEI) (Europe)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: Enhanced flow Polyetherimide copolymer (Tg 225C) with internal mold release and enhanced chemical resistance to strong acids, bases, aromatics and ketones. ECO Conforming.

Features: High Stiffness,Hydrolytic Stability,Enhanced Chemical Resistance,Easy Flow,Low Smoke and Toxicity,Good Mechanicals in Broad Temperature Range,Low Creep Sensitivity,Low Shrinkage,Good metal adhesion,Amorphous,High Strength,High Heat Resistance,Good dimensional stability,Flame Retardant,Good Mold Release

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.28 g/ccASTM D792
Density 1.28 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
 0.200 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 1.2 %ISO 62-1
Viscosity 20 cP
@Load 5.00 kg,
Temperature 360 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0040 - 0.0070 cm/cmSABIC method
 0.0040 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 11 g/10 min
@Load 6.60 kg,
Temperature 337 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 75.0 MPa5 mm/min; ASTM D638
 85.0 MPa5 mm/min; ISO 527
Tensile Strength, Yield 100 MPa5 mm/min; ASTM D638
 100 MPa5 mm/min; ISO 527
Elongation at Break 50 %5 mm/min; ISO 527
 60 %5 mm/min; ASTM D638
Elongation at Yield 8.0 %5 mm/min; ASTM D638
 8.0 %5 mm/min; ISO 527
Tensile Modulus 2900 MPa5 mm/min; ASTM D638
 2900 MPa1 mm/min; ISO 527
Flexural Strength 110 MPayield, 2 mm/min; ISO 178
 138 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2900 MPa2 mm/min; ISO 178
 3100 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 59.0 JASTM D256
 2080 J
@Thickness 3.20 mm
reverse notched; ASTM D256
Izod Impact, Unnotched 2100 J/mASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) NB80*10*4; ISO 180/1U
 NB
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched NBEdgew 80*10*4 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 7.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 30.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.50e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.2
@Frequency 50.0 - 60.0 Hz
ASTM D150
Dielectric Strength 18.0 kV/mm
@Thickness 3.20 mm
in oil; ASTM D149
 18.1 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
Dissipation Factor 0.0021
@Frequency 50.0 - 60.0 Hz
ASTM D150
 0.0021
@Frequency 50.0 - 60.0 Hz
IEC 60250
Comparative Tracking Index 100 VIEC 60112
 150 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 55.0 µm/m-°C
@Temperature -40.0 - 150 °C
ASTM E831
 55.0 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
CTE, linear, Transverse to Flow 55.0 µm/m-°C
@Temperature -40.0 - 150 °C
ASTM E831
 55.0 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Thermal Conductivity 0.310 W/m-KASTM C177
Hot Ball Pressure Test 125 °CPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 208 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 210 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
 213 °C
@Thickness 3.20 mm
unannealed; ASTM D648
 216 °C
@Thickness 6.40 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 198 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 200 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 201 °C
@Thickness 3.20 mm
unannealed; ASTM D648
 204 °C
@Thickness 6.40 mm
unannealed; ASTM D648
Vicat Softening Point 215 °CRate B/120; ISO 306
 215 °CRate B/50; ISO 306
 220 °CRate A/50; ISO 306
 227 °CRate B/50; ASTM D1525
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 360 - 380 °C
Zone 2 355 - 375 °C
Zone 3 365 - 390 °C
Melt Temperature 365 - 390 °CInjection Molding
Mold Temperature 135 - 165 °C
Drying Temperature 150 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
 24.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82684 / 290631

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.