MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Gougeon Brothers PRO-SET® INF-114/INF-211 Infusion Epoxy
Categories: Polymer; Thermoset; Epoxy

Material Notes: Very low viscosity for rapid saturation of fiberglass, Kevlar® and carbon fiber laminate with resin infusion and VARTM processes.
Medium cure speed hardener provides 3 to 4 hours working time at 77°F (25°C). A typical laminate will be gelled in 8 hours.
This combination is formulated specifically for resin infusion and VARTM processes. Do not use in open mold applications.
Room temperature cure properties suitable for many composite components and structures.
Tg as high as 196° F (91°C) with proper post cure providing excellent temperature stability and great part cosmetics.
Cost effective, high performance epoxy formulation for synthetic composite manufacturing.
Quality-control tinting is available at no extra charge; simply add "QC" after the product code on your order.

Information provided by Gougeon Brothers, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.930 g/ccHardener
 1.14 g/ccCured
 1.14 g/ccResin
Viscosity 14 cP
@Temperature 22.0 °C
hardener; ASTM D2196
 80 cP
@Temperature 48.9 °C
Mixed
 190 cP
@Temperature 29.4 °C
Mixed
 198 cP
@Temperature 29.0 °C
Mixed; ASTM D2196
 245 cP
@Temperature 25.0 °C
Mixed; ASTM D2196
 296 cP
@Temperature 22.0 °C
Mixed; ASTM D2196
 540 cP
@Temperature 15.6 °C
Mixed
 1433 cP
@Temperature 22.0 °C
resin; ASTM D2196
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 85
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
 85
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
 85
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
 86
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D2240
 86
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D2240
Tensile Strength 954 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 7770 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D638
 8540 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D638
 9820 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 10100 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Elongation at Break 1.7 %
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D638
 2.0 %
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D638
 2.6 %
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 3.9 %
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 5.3 %
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Tensile Modulus 487000 psiRT Gelation; ASTM D638
 511000 psiRT Gelation; ASTM D638
 524000 psiASTM D638
 534000 psiASTM D638
 535000 psiRT Gelation; ASTM D638
Flexural Strength 12300 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D790
 15000 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D790
 17100 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 17600 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 18200 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
Flexural Modulus 464000 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 483000 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D790
 485000 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D790
 495000 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 497000 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
Compressive Yield Strength 13700 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 13700 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 13700 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 14700 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D695
 15300 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D695
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 129 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D648
 131 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D648
 144 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
 160 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
 173 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
Glass Transition Temp, Tg 185 °FASTM E1356
 138 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DSC Onset– 1st Heat, 1 Hz, 3°C per minute; ASTM E1356
 138 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DSC Onset– 1st Heat, 1 Hz, 3°C per minute; ASTM E1356
 145 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DMA Onset Storage Modulus, 1 Hz, 3°C per minute; ASTM E1640
 145 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DMA Onset Storage Modulus, 1 Hz, 3°C per minute; ASTM E1640
 151 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 157 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DMA Peak Tan Delta, 1 Hz, 3°C per minute; ASTM E1640
 157 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 158 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DMA Peak Tan Delta, 1 Hz, 3°C per minute; ASTM E1640
 165 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 176 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 176 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 177 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 195 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 196 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 215 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 
Processing PropertiesOriginal ValueComments
Cure Time 8.00 hourtypical laminate will be gelled
Pot Life 56.0 - 70.0 min
@Load 0.500 kg,
Temperature 29.0 °C
ASTM D2471
 64.0 - 80.0 min
@Load 0.150 kg,
Temperature 29.0 °C
ASTM D2471
 76.0 - 94.0 min
@Load 0.500 kg,
Temperature 25.0 °C
ASTM D2471
 90.0 - 112 min
@Load 0.500 kg,
Temperature 22.0 °C
ASTM D2471
 109 - 135 min
@Load 0.150 kg,
Temperature 25.0 °C
ASTM D2471
 117 - 145 min
@Load 0.150 kg,
Temperature 22.0 °C
ASTM D2471
Working Life 3.00 - 4.00 hour
Shelf Life 24.0 Monthhardener
 36.0 Monthresin
 
Descriptive Properties
Mix ratio100:26.3–100:29.0Weight Range, Resin: Hardener
 100:27.4Weight, Resin: Hardener
 100:31.9–100:35.3Volume Range, Resin: Hardener
 100:33.3Volume, Resin: Hardener
 3.00:1Volume, Resin: Hardener
 3.13:1–2.84:1Volume Range, Resin: Hardener
 3.65:1Weight, Resin: Hardener
 3.81:1–3.45:1Weight Range, Resin: Hardener

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PGOUGP932 / 290775

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.