MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC LNP™ STAT-KON™ Compound DX11408 Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP STAT-KON DX11408 compound is based on Polycarbonate (PC) resin containing conductive carbon powder. Added features of this grade include: Electrically Conductive, Improved Ductility, meet ATEX requirements.

Features: Enhanced Ductility,Electrically Conductive

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.25 g/ccASTM D792
Density 1.25 g/ccASTM D792
Moisture Absorption 0.0200 %Injection Molding
 0.120 %23°C/50% RH/24 hrs; ASTM D570
 0.190 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0060 - 0.010 cm/cm24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0090 - 0.020 cm/cm24hrs; ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 48.0 MPa5 mm/min; ASTM D638
 48.0 MPa5 mm/min; ISO 527
Tensile Strength, Yield 55.0 MPa5 mm/min; ISO 527
 56.0 MPa5 mm/min; ASTM D638
Elongation at Break 16 %5 mm/min; ISO 527
 22 %5 mm/min; ASTM D638
Elongation at Yield 4.6 %5 mm/min; ISO 527
 4.7 %5 mm/min; ASTM D638
Tensile Modulus 2590 MPa5 mm/min; ASTM D638
 2630 MPa1 mm/min; ISO 527
Flexural Strength 88.0 MPaISO 178
Flexural Modulus 2480 MPa2 mm/min; ISO 178
 2680 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 337 JASTM D256
Izod Impact, Unnotched 940 J/mASTM D4812
Izod Impact, Notched (ISO) 21.0 kJ/m²80*10*4; ISO 180/1A
Dart Drop, Total Energy 38.0 JASTM D3763
Impact Test 34.0 JMultiaxial Impact; ISO 6603
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1000 - 1.00e+6 ohm-cmASTM D257
Surface Resistance 1000 - 1.00e+6 ohmASTM D257
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 62.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 136 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 137 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 127 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 130 °C
@Thickness 3.20 mm
unannealed; ASTM D648
UL RTI, Mechanical with Impact 115 °CUL 746B
UL RTI, Mechanical without Impact 115 °CUL 746B
Flammability, UL94 HB
@Thickness >=0.750 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Zone 2 310 - 320 °C
Zone 3 320 - 330 °C
Melt Temperature 305 - 325 °CInjection Molding
Mold Temperature 80.0 - 110 °C
Drying Temperature 120 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH81263 / 289210

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.