Physical Properties | Original Value | Comments |
---|
Density | 8.27 g/cc |
| 8.29 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength, Ultimate | 975 MPa @Treatment Temp. 871 °C, Time 3.60e+6 sec |
| 1102 MPa @Treatment Temp. 816 °C, Time 3.60e+6 sec |
| 1176 MPa @Treatment Temp. 760 °C, Time 3.60e+6 sec |
| 1191 MPa @Treatment Temp. 649 °C, Time 3.60e+6 sec |
Tensile Strength, Yield | 502 MPa @Treatment Temp. 502 °C, Time 3.60e+6 sec |
| 634 MPa @Treatment Temp. 634 °C, Time 3.60e+6 sec |
| 718 MPa @Treatment Temp. 718 °C, Time 3.60e+6 sec |
| 778 MPa @Treatment Temp. 778 °C, Time 3.60e+6 sec |
Elongation at Break | 22.3 % @Treatment Temp. 634 °C, Time 3.60e+6 sec |
| 22.8 % @Treatment Temp. 718 °C, Time 3.60e+6 sec |
| 24.2 % @Treatment Temp. 502 °C, Time 3.60e+6 sec |
| 25.8 % @Treatment Temp. 778 °C, Time 3.60e+6 sec |
Creep Strength | 34.0 MPa @Temperature 927 °C, Time 3.60e+6 sec |
| 62.0 MPa @Temperature 927 °C, Time 360000 sec |
| 69.0 MPa @Temperature 871 °C, Time 3.60e+6 sec |
| 124 MPa @Temperature 871 °C, Time 360000 sec |
| 145 MPa @Temperature 816 °C, Time 3.60e+6 sec |
| 221 MPa @Temperature 816 °C, Time 360000 sec |
| 241 MPa @Temperature 760 °C, Time 3.60e+6 sec |
| 331 MPa @Temperature 760 °C, Time 360000 sec |
| 365 MPa @Temperature 704 °C, Time 3.60e+6 sec |
| 496 MPa @Temperature 704 °C, Time 360000 sec |
| 545 MPa @Temperature 649 °C, Time 3.60e+6 sec |
Rupture Strength | 41.0 MPa @Temperature 927 °C, Time 3.60e+6 sec |
| 83.0 MPa @Temperature 927 °C, Time 360000 sec |
| 83.0 MPa @Temperature 871 °C, Time 3.60e+6 sec |
| 152 MPa @Temperature 871 °C, Time 360000 sec |
| 159 MPa @Temperature 816 °C, Time 3.60e+6 sec |
| 255 MPa @Temperature 816 °C, Time 360000 sec |
| 262 MPa @Temperature 760 °C, Time 3.60e+6 sec |
| 386 MPa @Temperature 760 °C, Time 360000 sec |
| 386 MPa @Temperature 704 °C, Time 3.60e+6 sec |
| 517 MPa @Temperature 704 °C, Time 360000 sec |
| 552 MPa @Temperature 649 °C, Time 3.60e+6 sec |
Modulus of Elasticity | 140 GPa @Temperature 1000 °C |
| 154 GPa @Temperature 900 °C |
| 166 GPa @Temperature 800 °C |
| 175 GPa @Temperature 700 °C |
| 183 GPa @Temperature 600 °C |
| 190 GPa @Temperature 500 °C |
| 196 GPa @Temperature 400 °C |
| 202 GPa @Temperature 300 °C |
| 209 GPa @Temperature 200 °C |
| 213 GPa @Temperature 100 °C |
| 217 GPa @Temperature 25.0 °C |
Poissons Ratio | 0.319 @Temperature 25.0 °C |
| 0.326 @Temperature 100 °C |
| 0.335 @Temperature 200 °C |
| 0.335 @Temperature 300 °C |
| 0.337 @Temperature 400 °C |
| 0.341 @Temperature 500 °C |
| 0.346 @Temperature 600 °C |
| 0.352 @Temperature 700 °C |
| 0.355 @Temperature 800 °C |
| 0.357 @Temperature 900 °C |
| 0.363 @Temperature 1000 °C |
Shear Modulus | 51.0 GPa @Temperature 1000 °C |
| 57.0 GPa @Temperature 900 °C |
| 61.0 GPa @Temperature 800 °C |
| 65.0 GPa @Temperature 700 °C |
| 68.0 GPa @Temperature 600 °C |
| 71.0 GPa @Temperature 500 °C |
| 73.0 GPa @Temperature 400 °C |
| 76.0 GPa @Temperature 300 °C |
| 78.0 GPa @Temperature 200 °C |
| 80.0 GPa @Temperature 100 °C |
| 82.0 GPa @Temperature 25.0 °C |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 0.0001261 ohm-cm @Temperature 25.0 °C |
| 0.0001278 ohm-cm @Temperature 100 °C |
| 0.0001299 ohm-cm @Temperature 200 °C |
| 0.0001299 ohm-cm @Temperature 1000 °C |
| 0.0001318 ohm-cm @Temperature 300 °C |
| 0.0001326 ohm-cm @Temperature 900 °C |
| 0.0001334 ohm-cm @Temperature 400 °C |
| 0.0001345 ohm-cm @Temperature 800 °C |
| 0.000135 ohm-cm @Temperature 500 °C |
| 0.0001355 ohm-cm @Temperature 700 °C |
| 0.0001362 ohm-cm @Temperature 600 °C |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 12.1 µm/m-°C @Temperature 25.0 - 100 °C |
| 12.4 µm/m-°C @Temperature 25.0 - 200 °C |
| 12.8 µm/m-°C @Temperature 25.0 - 300 °C |
| 13.1 µm/m-°C @Temperature 25.0 - 400 °C |
| 13.5 µm/m-°C @Temperature 25.0 - 500 °C |
| 13.7 µm/m-°C @Temperature 25.0 - 600 °C |
| 14.2 µm/m-°C @Temperature 25.0 - 700 °C |
| 14.9 µm/m-°C @Temperature 25.0 - 800 °C |
| 15.9 µm/m-°C @Temperature 25.0 - 900 °C |
| 16.9 µm/m-°C @Temperature 25.0 - 1000 °C |
Specific Heat Capacity | 0.436 J/g-°C @Temperature 25.0 °C |
| 0.463 J/g-°C @Temperature 100 °C |
| 0.494 J/g-°C @Temperature 200 °C |
| 0.522 J/g-°C @Temperature 300 °C |
| 0.544 J/g-°C @Temperature 400 °C |
| 0.563 J/g-°C @Temperature 500 °C |
| 0.581 J/g-°C @Temperature 600 °C |
| 0.594 J/g-°C @Temperature 700 °C |
| 0.650 J/g-°C @Temperature 800 °C |
| 0.668 J/g-°C @Temperature 900 °C |
| 0.676 J/g-°C @Temperature 1000 °C |
Thermal Conductivity | 10.3 W/m-K @Temperature 25.0 °C |
| 12.0 W/m-K @Temperature 100 °C |
| 14.1 W/m-K @Temperature 200 °C |
| 16.3 W/m-K @Temperature 300 °C |
| 18.5 W/m-K @Temperature 400 °C |
| 20.5 W/m-K @Temperature 500 °C |
| 22.6 W/m-K @Temperature 600 °C |
| 24.8 W/m-K @Temperature 700 °C |
| 26.1 W/m-K @Temperature 800 °C |
| 27.3 W/m-K @Temperature 900 °C |
| 28.9 W/m-K @Temperature 1000 °C |
Melting Point | 1300 - 1375 °C |
Solidus | 1300 °C |
Liquidus | 1375 °C |
|
Processing Properties | Original Value | Comments |
---|
Annealing Temperature | 2050 - 2100 °F |
|
Component Elements Properties | Original Value | Comments |
---|
Aluminum, Al | 1.5 % |
Boron, B | 0.0050 % |
Carbon, C | 0.060 % |
Chromium, Cr | 20 % |
Cobalt, Co | 10 % |
Iron, Fe | <= 1.5 % |
Manganese, Mn | <= 0.30 % |
Molybdenum, Mo | 8.5 % |
Nickel, Ni | 57 % |
Silicon, Si | <= 0.15 % |
Titanium, Ti | 2.1 % |
|
Descriptive Properties |
---|
Thermal Diffusivity | 0.0288 cm2/s |
| 0.0315 cm2/s |
| 0.0348 cm2/s |
| 0.0381 cm2/s |
| 0.0413 cm2/s |
| 0.0444 cm2/s |
| 0.0473 cm2/s |
| 0.0488 cm2/s |
| 0.0498 cm2/s |
| 0.0509 cm2/s |
| 0.0521 cm2/s |