MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Copper Alloy, UNS C69430, O60 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Soft Anneal

Fabrication Properties: Excellent Suitability – Soldering, Brazing, Capacity for Being Hot Formed; Good Suitability – Oxyacetylene Welding, Spot Weld, Seam Weld, Butt Weld, Capacity for Being Cold Worked

Common Fabrication Processes: Forging; Screw Machining

Typical uses: Valve Stems

Applicable Specifications: Rod – ASTM B371/B371M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.260 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 85
@Thickness 50.8 mm
 85
@Thickness 25.4 mm
 85
@Thickness 12.7 mm
Tensile Strength 80.0 ksi
@Thickness 50.8 mm
 85.0 ksi
@Thickness 25.4 mm
 90.0 ksi
@Thickness 12.7 mm
Tensile Strength, Yield 40.0 ksi
@Thickness 50.8 mm
0.5% Ext
 43.0 ksi
@Thickness 25.4 mm
0.5% Ext
 45.0 ksi
@Thickness 12.7 mm
0.5% Ext
Elongation at Break 20 %
@Thickness 12.7 mm
 25 %
@Thickness 50.8 mm
 25 %
@Thickness 25.4 mm
Tensile Modulus 16000 ksi
Machinability 30 %
Forgeability 80 %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000280 ohm-cm6.2% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.2 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 15.0 BTU-in/hr-ft²-°F
Melting Point 1510 - 1685 °F
Solidus 1510 °F
Liquidus 1685 °F
 
Component Elements PropertiesOriginal ValueComments
Arsenic, As 0.030 - 0.060 %
Copper, Cu 80 - 83 %
Iron, Fe <= 0.20 %
Lead, Pb <= 0.30 %
Silicon, Si 3.5 - 4.5 %
Zinc, Zn 12.1 - 16.5 %As Balance

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC69430x2 / 292385

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.