MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Plenco PlasGlas™ 10313 General Purpose Thermoset Polyester BMC  (discontinued **)
Categories: Polymer; Thermoset; Polyester, TS; Thermoset Polyester Glass Filled BMC

Material Notes: PlasGlas 10313 is a general purpose polyester bulk molding compound that is characterized by adding utility to a number of applications. Because of its combination of high heat resistance, good electrical properties, flame resistance and strength, it can be used in such applications as iron skirts and other small appliance housings, coil bobbins, and electric motor components such as brush holders. It is available in either bulk or extruded form and is currently available in black. Other colors are available upon request.

Data provided by Plaslok Corporation.

Plaslok Corporation was purchased by Plastics Engineering Company in March 2000. The Plaslok name is no longer used on any products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.85 g/ccASTM D792
Water Absorption 0.080 %ASTM D570
Linear Mold Shrinkage 0.0020 cm/cmCompression; ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 40ASTM D2583
Tensile Strength, Ultimate 44.0 MPaASTM D638
Flexural Yield Strength 104 MPaASTM D790
Flexural Modulus 21.0 GPaASTM D790
Compressive Yield Strength 117 MPaASTM D695
Izod Impact, Notched 3.20 J/cmASTM D256
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 4.3
@Frequency 1e+6 Hz
ASTM D150
 5.7
@Frequency 60 Hz
ASTM D150
Dielectric Strength 13.8 kV/mmASTM D149
Dissipation Factor 0.020
@Frequency 60 Hz
ASTM D150
 0.080
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance >= 190 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) >= 260 °CASTM D648
UL RTI, Electrical 130 °C
@Thickness 1.50 mm
UL RTI, Mechanical with Impact 130 °C
@Thickness 1.50 mm
UL RTI, Mechanical without Impact 130 °C
@Thickness 1.50 mm
Flammability, UL94 V-0
@Thickness 1.50 mm
 V-0
@Thickness 1.50 mm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PLEO926 / 50814

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.