MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
BASF Ultraform® N 2200 G53 UNC Q600 25% Glass Filled POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, 30% Glass Fiber Reinforced

Material Notes: Ultraform N2200 G53 UNC Q600 is a 25% glass fiber reinforced POM injection molding grade with enhanced stiffness and toughness.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.58 g/ccISO 1183
Water Absorption 0.90 %ISO 62
Moisture Absorption at Equilibrium 0.15 %23°C/50% R.H.; ISO 62
Melt Flow 5.5 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 190 MPaISO2039
Tensile Strength at Break 130 MPa5mm/min; ISO 527
Tensile Strength, Yield 60.0 MPa
@Temperature 120 °C
ISO 527
 90.0 MPa
@Temperature 80.0 °C
ISO 527
 125 MPa
@Temperature 40.0 °C
ISO 527
Tensile Stress at Strain 10.0 MPa
@Strain 0.2 %,
Time 3.60e+7 sec
ISO 899-1
 12.0 MPa
@Strain 0.2 %,
Time 3.60e+6 sec
ISO 899-1
 15.0 MPa
@Strain 0.2 %,
Time 3600 sec
ISO 899-1
 31.0 MPa
@Strain 0.6 %,
Time 3.60e+6 sec
ISO 899-1
 32.0 MPa
@Strain 0.6 %,
Time 3.60e+7 sec
ISO 899-1
 35.0 MPa
@Strain 0.5 %,
Time 3600 sec
ISO 899-1
 55.0 MPa
@Strain 1.4 %,
Time 3.60e+6 sec
ISO 899-1
 55.0 MPa
@Strain 1.8 %,
Time 3.60e+7 sec
ISO 899-1
 58.0 MPa
@Strain 0.8 %,
Time 3600 sec
ISO 899-1
Elongation at Break 3.0 %5mm/min; ISO 527
Modulus of Elasticity 8.80 GPaISO 527
 2.50 GPa
@Temperature 140 °C
SIO 527
 5.00 GPa
@Temperature 100 °C
SIO 527
 8.10 GPa
@Temperature 40.0 °C
SIO 527
Izod Impact, Notched (ISO) 9.00 kJ/m²ISO 180
 9.00 kJ/m²
@Temperature -30.0 °C
ISO 180
Charpy Impact Unnotched 5.50 J/cm²ISO 179
 6.00 J/cm²
@Temperature -30.0 °C
ISO 179
Charpy Impact, Notched 0.900 J/cm²ISO 179
 0.880 J/cm²
@Temperature -30.0 °C
ISO 179
Tensile Creep Modulus, 1000 hours 5800 MPaISO 899
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+12 ohm-cmIEC 60093
Surface Resistance 1.00e+14 ohmIEC 60093
Dielectric Constant 4.0
@Frequency 100 Hz
IEC 60250
 4.0
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 43.0 kV/mmIEC 60243-1
Dissipation Factor 0.0040
@Frequency 100 Hz
IEC 60250
 0.0070
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VTest Solution A; IEC 60112
 600 VTest Solution B; IEC 60112
 
Thermal PropertiesOriginal ValueComments
Melting Point 168 °CDIN 53765
Maximum Service Temperature, Air 110 °C
Deflection Temperature at 1.8 MPa (264 psi) 163 °CISO 75
Vicat Softening Point 160 °C(50 °C/h / 50N) - B/50; ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 190 - 230 °C
Mold Temperature 60.0 - 120 °C
 
Descriptive Properties
ColorNatural
Commercial StatusActive America
Impact ModifiedNo
Primary Processing TechniqueInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultraform® N2720 M63 30% Mineral Filled POM
BASF Ultraform® H 2320 006 Q600 POM
BASF Ultraform® FK 61002 20% Carbon Black Filled POM
Delrin Delrin® 525GR BK000 POM-GF25
BASF Ultraform® N2200 G43 POM

PBASF9101 / 84865

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.