MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Outokumpu LDX 2101® Duplex Stainless Steel
Categories: Metal; Ferrous Metal; Duplex; Stainless Steel

Material Notes:

Applications:

  • Pulp and paper industry
  • Desalination plants
  • Flue-gas cleaning
  • Cargo tanks and pipe systems in chemical tankers
  • Seawater systems
  • Firewalls and blast walls on offshore platforms
  • Bridges
  • Components for structural design
  • Storage tanks
  • Pressure vessels
  • Heat exchangers
  • Water heaters
  • Rotors, impellers and shafts

Available in hot rolled plate (Quarto), hot rolled strip/sheet (CPP), cold rolled strip/sheet, and rod forms.

Key Words: EN 1.4162; UNS S32101
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/ccRT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 700 MPaOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 540 MPa
@Temperature 200 °C
EN min.; EN 10002-5
 540 MPa
@Temperature 250 °C
EN min.; EN 10002-5
 560 MPa
@Temperature 150 °C
EN min.; EN 10002-5
 590 MPa
@Temperature 100 °C
EN min.; EN 10002-5
Tensile Strength, Yield 450 MPa
@Strain 0.2 %
EN min., RT; EN 10002-1
 480 MPa
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 320 MPa
@Strain 0.2 %,
Temperature 250 °C
EN min.; EN 10002-5
 330 MPa
@Strain 0.2 %,
Temperature 200 °C
EN min.; EN 10002-5
 350 MPa
@Strain 0.2 %,
Temperature 150 °C
EN min.; EN 10002-5
 380 MPa
@Strain 0.2 %,
Temperature 100 °C
EN min.; EN 10002-5
Elongation at Break 38 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
Modulus of Elasticity 200 GPaRT
 172 GPa
@Temperature 400 °C
 180 GPa
@Temperature 300 °C
 186 GPa
@Temperature 200 °C
 194 GPa
@Temperature 100 °C
Poissons Ratio 0.30RT
Fatigue Strength 500 MPa
@# of Cycles 2.00e+6
R=smin/smax=0.1;RT; 50% probability of failure
 696 MPa
@# of Cycles 2.00e+6
R=smin/smax=0.1; F50
 478 MPa
@Strain 0.2 %
R=smin/smax=0.1; 2 million cycles, F50
Shear Modulus 77.0 GPacalculated
Impact Test >= 60.0 JTransverse Direction, from AM 611; EN 10045-1
 >= 27.0 J
@Temperature -40.0 °C
from AM 611; EN 10045-1
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000800 ohm-cmRT
 0.0000850 ohm-cm
@Temperature 100 °C
 0.0000900 ohm-cm
@Temperature 200 °C
 0.000100 ohm-cm
@Temperature 300 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.0 µm/m-°C
@Temperature 100 °C
 14.5 µm/m-°C
@Temperature 400 °C
Specific Heat Capacity 0.500 J/g-°CRT
 0.530 J/g-°C
@Temperature 100 °C
 0.560 J/g-°C
@Temperature 200 °C
 0.590 J/g-°C
@Temperature 300 °C
Thermal Conductivity 15.0 W/m-KRT
 16.0 W/m-K
@Temperature 100 °C
 17.0 W/m-K
@Temperature 200 °C
 18.0 W/m-K
@Temperature 300 °C
 20.0 W/m-K
@Temperature 400 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 1020 - 1080 °CQuench Annealing
 1020 - 1080 °CStress Relief Annealing
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.030 %
Chromium, Cr 21.5 %
Iron, Fe 71.45 %
Manganese, Mn 5.0 %
Molybdenum, Mo 0.30 %
Nickel, Ni 1.5 %
Nitrogen, N 0.22 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Outokumpu 2205 Duplex Stainless Steel
Sandvik LDX 2101 Plate and sheet
Outokumpu SAF 2304® Duplex Stainless Steel
Outokumpu SAF 2507® Duplex Stainless Steel
AISI Type 430F Stainless Steel

NOUTOK04 / 18719

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.