MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC XYLEX™ X7300 PC+Polyester (Americas)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/PET Polyester Blend

Material Notes: PC+POLYESTER unreinforced alloy. High flow, chemically resistant with excellent optical quality. UV-stabilized.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
Density 1.18 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 21 g/10 min
@Load 2.16 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 21 g/10 min
@Load 2.16 kg,
Temperature 265 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 52.0 MPa50 mm/min; ASTM D638
 55.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 49.0 MPa50 mm/min; ASTM D638
 55.0 MPa50 mm/min; ISO 527
Elongation at Break >= 150 %50mm/min; ISO 527
 150 %50 mm/min; ASTM D638
Elongation at Yield 5.0 %50 mm/min; ASTM D638
 5.0 %50 mm/min; ISO 527
Tensile Modulus 1840 MPa50 mm/min; ASTM D638
 1900 MPa1mm/min; ISO 527
Flexural Strength 71.0 MPa2 mm/min; break; ISO 178
Flexural Yield Strength 83.0 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 1940 MPa1.3 mm/min, 50 mm span; ASTM D790
 2000 MPa2 mm/min; ISO 178
Izod Impact, Notched 660 J/mASTM D256
Izod Impact, Notched (ISO) 9.00 kJ/m²80*10*4; ISO 180/1A
Dart Drop, Total Energy 95.0 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 85.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
 115 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
CTE, linear, Transverse to Flow 85.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
 105 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 102 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °C1.8 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
 88.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 106 °CRate B/120; ISO 306
 108 °CRate B/50; ASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 2.0 %
@Thickness 2.54 mm
ASTM D1003
Transmission, Visible 88 %
@Thickness 2.54 mm
ASTM D1003
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 250 - 270 °CInjection Molding
Zone 1 240 - 250 °C
Zone 2 245 - 265 °C
Zone 3 250 - 270 °C
Melt Temperature 250 - 270 °C
Mold Temperature 45.0 - 60.0 °C
Drying Temperature 80.0 - 95.0 °CInjection Molding
Dry Time 3.00 - 5.00 hourInjection Molding
 8.00 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.200 - 0.500 MPa
Shot Size 40 - 80 %
Vent Depth 0.00130 - 0.00200 cm
Screw Speed 20 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI11626 / 245093

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.