MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

(Viewing data as-entered. Click here to return)
Haynes 282® Nickel Alloy Plate, Solution Annealed and Age-Hardened, after long term high temperature exposure
Categories: Metal; Nonferrous Metal; Nickel Alloy

Material Notes: Excellent High Temperature Strength

HAYNES® 282® alloy is a wrought, gamma-prime strengthened superalloy developed for high temperature structural applications, especially those in aero and land-based gas turbine engines. It possesses a unique combination of creep strength, thermal stability, weldability, and fabricability. The alloy has excellent creep strength in the temperature range of 1200 to 1700°F (649 to 927°C), surpassing that of Waspaloy alloy, and approaching that of R-41 alloy.

Easily Fabricated: This high level of creep strength in HAYNES 282 alloy has been attained at a relatively low volume fraction of the strengthening gamma-prime phase, resulting in outstanding resistance to strain-age cracking (normally a problem with superalloys in this creep strength range). Additionally, slow gamma-prime precipitation kinetics allow for the alloy to have excellent ductility in the as-annealed condition. Consequently, HAYNES 282 alloy exhibits superior weldability and fabricability.

Product Forms: HAYNES 282 alloy is designed for use in the form of plate, sheet, strip, foil, billet, bar, wire welding products, pipe, and tubing.

Heat Treatment: HAYNES 282 alloy is provided in the solution-annealed condition, in which it is readily formable. The typical solution annealing temperature is in the range of 2050 to 2100°F (1121 to 1149°C). After component fabrication, a two-step age hardening treatment is required to put the alloy into the high-strength condition. The treatment includes 1850°F (1010°C) / 2 hours / AC (air cool) + 1450°F (788°C) / 8 hours / AC.

Applications: Suitable for critical gas turbine applications, such as sheet fabrications, seamless and flash butt-welded rings, and cases found in compressor, combustor, and turbine sections. In augmented aircraft gas turbines, it is useful for exhaust and nozzle components. In land-based gas turbines, HAYNES 282 alloy is a good candidate for transition sections and other hot-gas-path components.

Machining: HAYNES 282 alloy has similar machining characteristics to other nickel alloys used at high temperatures. Rough machining should be carried out prior to age-hardening, using the following guidelines. Final machining or finish grinding may be done after age-hardening.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.27 g/ccSolution Annealed
 8.29 g/ccAge-hardened
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1152 MPaRoom temp test prior to thermal exposure
 978 MPa
@Treatment Temp. 871 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 1006 MPa
@Treatment Temp. 871 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 1022 MPa
@Treatment Temp. 871 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 1065 MPa
@Treatment Temp. 871 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 1114 MPa
@Treatment Temp. 871 °C,
Time 360000 sec
Room temp test after thermal exposure
 1161 MPa
@Treatment Temp. 760 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 1191 MPa
@Treatment Temp. 760 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 1205 MPa
@Treatment Temp. 760 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 1223 MPa
@Treatment Temp. 760 °C,
Time 360000 sec
Room temp test after thermal exposure
 1226 MPa
@Treatment Temp. 760 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 1247 MPa
@Treatment Temp. 649 °C,
Time 360000 sec
Room temp test after thermal exposure
 1248 MPa
@Treatment Temp. 649 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 1255 MPa
@Treatment Temp. 649 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 1260 MPa
@Treatment Temp. 649 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 1264 MPa
@Treatment Temp. 649 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
Tensile Strength, Yield 705 MPa0.2%. Room temp test prior to thermal exposure
 452 MPa
@Treatment Temp. 871 °C,
Time 5.76e+7 sec
0.2%. Room temp test after thermal exposure
 473 MPa
@Treatment Temp. 871 °C,
Time 2.88e+7 sec
0.2%. Room temp test after thermal exposure
 487 MPa
@Treatment Temp. 871 °C,
Time 1.44e+7 sec
0.2%. Room temp test after thermal exposure
 533 MPa
@Treatment Temp. 871 °C,
Time 3.60e+6 sec
0.2%. Room temp test after thermal exposure
 618 MPa
@Treatment Temp. 871 °C,
Time 360000 sec
0.2%. Room temp test after thermal exposure
 658 MPa
@Treatment Temp. 760 °C,
Time 5.76e+7 sec
0.2%. Room temp test after thermal exposure
 690 MPa
@Treatment Temp. 760 °C,
Time 2.88e+7 sec
0.2%. Room temp test after thermal exposure
 707 MPa
@Treatment Temp. 760 °C,
Time 1.44e+7 sec
0.2%. Room temp test after thermal exposure
 742 MPa
@Treatment Temp. 760 °C,
Time 3.60e+6 sec
0.2%. Room temp test after thermal exposure
 759 MPa
@Treatment Temp. 760 °C,
Time 360000 sec
0.2%. Room temp test after thermal exposure
 798 MPa
@Treatment Temp. 649 °C,
Time 360000 sec
0.2%. Room temp test after thermal exposure
 814 MPa
@Treatment Temp. 649 °C,
Time 3.60e+6 sec
0.2%. Room temp test after thermal exposure
 816 MPa
@Treatment Temp. 649 °C,
Time 5.76e+7 sec
0.2%. Room temp test after thermal exposure
 819 MPa
@Treatment Temp. 649 °C,
Time 2.88e+7 sec
0.2%. Room temp test after thermal exposure
 830 MPa
@Treatment Temp. 649 °C,
Time 1.44e+7 sec
0.2%. Room temp test after thermal exposure
Elongation at Break 30 %Room temp test prior to thermal exposure
 20 %
@Treatment Temp. 760 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 20 %
@Treatment Temp. 760 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 21 %
@Treatment Temp. 760 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 23 %
@Treatment Temp. 649 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 24 %
@Treatment Temp. 649 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 26 %
@Treatment Temp. 649 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 26 %
@Treatment Temp. 649 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 26 %
@Treatment Temp. 760 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 27 %
@Treatment Temp. 649 °C,
Time 360000 sec
Room temp test after thermal exposure
 27 %
@Treatment Temp. 760 °C,
Time 360000 sec
Room temp test after thermal exposure
 30 %
@Treatment Temp. 871 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 31 %
@Treatment Temp. 871 °C,
Time 360000 sec
Room temp test after thermal exposure
 32 %
@Treatment Temp. 871 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 32 %
@Treatment Temp. 871 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 33 %
@Treatment Temp. 871 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
Reduction of Area 33 %Room temp test prior to thermal exposure
 19 %
@Treatment Temp. 760 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 21 %
@Treatment Temp. 760 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 22 %
@Treatment Temp. 760 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 25 %
@Treatment Temp. 649 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 27 %
@Treatment Temp. 649 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 29 %
@Treatment Temp. 649 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 29 %
@Treatment Temp. 649 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 29 %
@Treatment Temp. 760 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 30 %
@Treatment Temp. 760 °C,
Time 360000 sec
Room temp test after thermal exposure
 30 %
@Treatment Temp. 871 °C,
Time 3.60e+6 sec
Room temp test after thermal exposure
 31 %
@Treatment Temp. 649 °C,
Time 360000 sec
Room temp test after thermal exposure
 31 %
@Treatment Temp. 871 °C,
Time 1.44e+7 sec
Room temp test after thermal exposure
 31 %
@Treatment Temp. 871 °C,
Time 2.88e+7 sec
Room temp test after thermal exposure
 32 %
@Treatment Temp. 871 °C,
Time 5.76e+7 sec
Room temp test after thermal exposure
 36 %
@Treatment Temp. 871 °C,
Time 360000 sec
Room temp test after thermal exposure
Modulus of Elasticity 217 GPa
@Temperature 25.0 °C
Dynamic
Poissons Ratio 0.319
@Temperature 25.0 °C
Shear Modulus 82.0 GPa
@Temperature 25.0 °C
Dynamic
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0001278 ohm-cm
 0.0001299 ohm-cm
 0.0001299 ohm-cm
 0.0001318 ohm-cm
 0.0001326 ohm-cm
 0.0001334 ohm-cm
 0.0001345 ohm-cm
 0.000135 ohm-cm
 0.0001355 ohm-cm
 0.0001362 ohm-cm
 0.0001261 ohm-cm
@Temperature 25.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.1 µm/m-°C
@Temperature 25.0 - 100 °C
Specific Heat Capacity 0.436 J/g-°C
@Temperature 25.0 °C
Thermal Conductivity 10.3 W/m-K
@Temperature 25.0 °C
Melting Point 1300 - 1375 °C
Solidus 1300 °C
Liquidus 1375 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 2050 - 2100 °FTypical for solution annealing
Aging Temperature 1450 °F
@Time 28800 sec
Age Hardening Step 2 of 2, with subsequent air cooling
 1850 °F
@Time 7200 sec
Age Hardening Step 1 of 2, with subsequent air cooling
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 1.5 %
Boron, B 0.0050 %
Carbon, C 0.060 %
Chromium, Cr 20 %
Cobalt, Co 10 %
Iron, Fe <= 1.5 %
Manganese, Mn <= 0.30 %
Molybdenum, Mo 8.5 %
Nickel, Ni 57 %as balance
Silicon, Si <= 0.15 %
Titanium, Ti 2.1 %
 
Descriptive Properties
Thermal Diffusivity0.0288 cm2/s25°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals NIMONIC® Alloy 90
Special Metals INCONEL® Alloy 718
Special Metals INCONEL® 625LCF® Nickel Superalloy (UNS N06626) Annealed 1950°F (1070°C) + Aged 1400°F (760°C)
Special Metals INCONEL® Alloy X-750
Haynes 282® Nickel Alloy Plate, Solution Annealed and Age-Hardened

NHAY987a / 162652

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.