MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Gougeon Brothers PRO-SET® LAM-145/LAM-226 Laminating Epoxy
Categories: Polymer; Thermoset; Epoxy

Material Notes: Medium viscosity for good wet out of all synthetic composite fabrics and core materials.
Thixotropic to prevent drain out in heavy fabrics and on vertical surfaces.
High tack to help hold heavy fabric and core in place on vertical surfaces.
Medium cure speed hardener provides 2 to 3 hours of working time at 77°F (25°C). A typical laminate will be gelled in 4 to 5 hours.
Optimized for hand wet out and machine impregnation in contact molding, vacuum bagging and filament winding applications.
Room temperature cure properties suitable for many composite components and structures.
Tg as high as 219°F (104°C) with proper post cure providing excellent temperature stability and great part cosmetics.
Cost effective, high performance epoxy formulation for synthetic composite manufacturing.
Quality-control tinting is available at no extra charge; simply add "QC" after the produce code on your order.

Information provided by Gougeon Brothers, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.970 g/ccHardener
 1.16 g/ccCured
 1.17 g/ccResin
Viscosity 42 cP
@Temperature 22.0 °C
hardener; ASTM D2196
 400 cP
@Temperature 48.9 °C
Mixed
 1076 cP
@Temperature 29.0 °C
Mixed; ASTM D2196
 1200 cP
@Temperature 29.4 °C
Mixed
 1455 cP
@Temperature 25.0 °C
Mixed; ASTM D2196
 1868 cP
@Temperature 22.0 °C
Mixed; ASTM D2196
 3600 cP
@Temperature 15.6 °C
Mixed
 10000 cP
@Temperature 22.0 °C
resin; ASTM D2196
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 90
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
 91
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D2240
 92
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D2240
 92
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
 94
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D2240
Tensile Strength 8600 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D638
 9560 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D638
 11000 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 11000 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 11000 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Elongation at Break 1.7 %
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D638
 2.1 %
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D638
 3.6 %
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 4.4 %
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
 5.9 %
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D638
Tensile Modulus 445000 psiRT Gelation; ASTM D638
 491000 psiRT Gelation; ASTM D638
 507000 psiRT Gelation; ASTM D638
 535000 psiASTM D638
 582000 psiASTM D638
Flexural Strength 14600 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D790
 15100 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D790
 19700 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 20000 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 20300 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
Flexural Modulus 469000 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 518000 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 548000 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D790
 570000 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D790
 575000 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D790
Compressive Yield Strength 14900 psi
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 14900 psi
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 14900 psi
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D695
 15700 psi
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D695
 16100 psi
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D695
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 129 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
ASTM D648
 129 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
ASTM D648
 154 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
 166 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
 198 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
RT Gelation; ASTM D648
Glass Transition Temp, Tg 208 °FASTM E1356
 134 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DSC Onset– 1st Heat, 1 Hz, 3°C per minute; ASTM E1356
 134 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DSC Onset– 1st Heat, 1 Hz, 3°C per minute; ASTM E1356
 144 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DMA Onset Storage Modulus, 1 Hz, 3°C per minute; ASTM E1640
 148 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DMA Onset Storage Modulus, 1 Hz, 3°C per minute; ASTM E1640
 156 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 160 °F
@Treatment Temp. 22.0 °C,
Time 2.42e+6 sec
DMA Peak Tan Delta, 1 Hz, 3°C per minute; ASTM E1640
 163 °F
@Treatment Temp. 25.0 °C,
Time 1.21e+6 sec
DMA Peak Tan Delta, 1 Hz, 3°C per minute; ASTM E1640
 169 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 171 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 186 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 188 °F
@Treatment Temp. 49.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 198 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DSC Onset– 1st Heat, RT Gelation, 1 Hz, 3°C per minute; ASTM E1356
 206 °F
@Treatment Temp. 60.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 219 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DMA Onset Storage Modulus, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 236 °F
@Treatment Temp. 82.0 °C,
Time 28800 sec
DMA Peak Tan Delta, RT Gelation, 1 Hz, 3°C per minute; ASTM E1640
 
Processing PropertiesOriginal ValueComments
Cure Time 4.00 - 5.00 hourtypical laminate will be gelled
Pot Life 33.0 - 41.0 min
@Load 0.500 kg,
Temperature 29.0 °C
ASTM D2471
 36.0 - 43.0 min
@Load 0.500 kg,
Temperature 22.0 °C
ASTM D2471
 36.0 - 46.0 min
@Load 0.150 kg,
Temperature 29.0 °C
ASTM D2471
 38.0 - 48.0 min
@Load 0.500 kg,
Temperature 25.0 °C
ASTM D2471
 44.0 - 54.0 min
@Load 0.150 kg,
Temperature 25.0 °C
ASTM D2471
 52.0 - 64.0 min
@Load 0.150 kg,
Temperature 22.0 °C
ASTM D2471
Working Life 2.00 - 3.00 hour
Shelf Life 24.0 Monthhardener
 36.0 Monthresin
 
Descriptive Properties
Mix ratio100:26.2–100:30.4Weight Range, Resin: Hardener
 100:27.6Weight, Resin: Hardener
 100:31.6–100:36.7Volume Range, Resin: Hardener
 100:33.3Volume, Resin: Hardener
 3.00:1Volume, Resin: Hardener
 3.16:1–2.72:1Volume Range, Resin: Hardener
 3.5:1Weight, Resin: Hardener
 3.82:1–3.29:1Weight Range, Resin: Hardener

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PGOUGP920 / 290763

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.