MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
416 Stainless Steel
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes: 25 mm diameter bar, oil quenched from 995°C, held at tempering temperature for 2 hours.

Key Words: UNS S41600, ASME SA194, ASTM A194, ASTM A314, ASTM A473, ASTM A581, ASTM A582, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405(51416), DIN 1.4005, UNI X 12 CrS 13, B.S. 416 S 21, martensitic, ISO 683/13 7
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 237
@Temperature 705 °C
Converted from Rockwell C Hardness
 253
@Temperature 650 °C
Converted from Rockwell C Hardness
 266
@Temperature 595 °C
Converted from Rockwell C Hardness
 318
@Temperature 540 °C
Converted from Rockwell C Hardness
 360
@Temperature 260 °C
Converted from Rockwell C Hardness
 360
@Temperature 370 °C
Converted from Rockwell C Hardness
 360
@Temperature 480 °C
Converted from Rockwell C Hardness
 365
@Temperature 150 °C
Converted from Rockwell C Hardness
Hardness, Knoop 250
@Temperature 705 °C
Converted from Rockwell C Hardness
 268
@Temperature 650 °C
Converted from Rockwell C Hardness
 283
@Temperature 595 °C
Converted from Rockwell C Hardness
 343
@Temperature 540 °C
Converted from Rockwell C Hardness
 392
@Temperature 260 °C
Converted from Rockwell C Hardness
 392
@Temperature 370 °C
Converted from Rockwell C Hardness
 392
@Temperature 480 °C
Converted from Rockwell C Hardness
 397
@Temperature 150 °C
Converted from Rockwell C Hardness
Hardness, Rockwell C 20
@Temperature 705 °C
 23.5
@Temperature 650 °C
 26
@Temperature 595 °C
 34
@Temperature 540 °C
 39
@Temperature 260 °C
 39
@Temperature 370 °C
 39
@Temperature 480 °C
 39.5
@Temperature 150 °C
Hardness, Vickers 242
@Temperature 705 °C
Converted from Rockwell C Hardness
 260
@Temperature 650 °C
Converted from Rockwell C Hardness
 275
@Temperature 595 °C
Converted from Rockwell C Hardness
 332
@Temperature 540 °C
Converted from Rockwell C Hardness
 378
@Temperature 260 °C
Converted from Rockwell C Hardness
 378
@Temperature 370 °C
Converted from Rockwell C Hardness
 378
@Temperature 480 °C
Converted from Rockwell C Hardness
 383
@Temperature 150 °C
Converted from Rockwell C hardness.
Tensile Strength, Ultimate 741 MPa
@Temperature 705 °C
 796 MPa
@Temperature 650 °C
 865 MPa
@Temperature 595 °C
 1080 MPa
@Temperature 540 °C
 1185 MPa
@Temperature 480 °C
 1260 MPa
@Temperature 370 °C
 1295 MPa
@Temperature 260 °C
 1310 MPa
@Temperature 150 °C
Tensile Strength, Yield 600 MPa
@Strain 0.2 %,
Temperature 705 °C
 670 MPa
@Strain 0.2 %,
Temperature 650 °C
 740 MPa
@Strain 0.2 %,
Temperature 595 °C
 895 MPa
@Strain 0.2 %,
Temperature 540 °C
 962 MPa
@Strain 0.2 %,
Temperature 150 °C
 962 MPa
@Strain 0.2 %,
Temperature 260 °C
 962 MPa
@Strain 0.2 %,
Temperature 370 °C
 983 MPa
@Strain 0.2 %,
Temperature 480 °C
Elongation at Break 9.0 %
@Temperature 150 °C
in 50 mm
 9.5 %
@Temperature 260 °C
in 50 mm
 13 %
@Temperature 540 °C
in 50 mm
 14 %
@Temperature 370 °C
in 50 mm
 16 %
@Temperature 480 °C
in 50 mm
 17 %
@Temperature 595 °C
in 50 mm
 17.5 %
@Temperature 650 °C
in 50 mm
 20 %
@Temperature 705 °C
in 50 mm
Modulus of Elasticity 200 GPa
Poissons Ratio 0.20Calculated
Shear Modulus 83.0 GPa
Izod Impact 20.3 J
@Temperature 150 °C
 20.3 J
@Temperature 260 °C
 20.3 J
@Temperature 370 °C
 20.3 J
@Temperature 480 °C
 27.3 J
@Temperature 540 °C
 54.4 J
@Temperature 595 °C
 61.1 J
@Temperature 650 °C
 75.0 J
@Temperature 705 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000570 ohm-cm
@Temperature 20.0 °C
 0.000108 ohm-cm
@Temperature 650 °C
Magnetic Permeability 700 - 1000annealed condition at RT
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.90 µm/m-°C
@Temperature 0.000 - 100 °C
 11.0 µm/m-°C
@Temperature 0.000 - 315 °C
 11.5 µm/m-°C
@Temperature 0.000 - 540 °C
 11.7 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 24.9 W/m-K
@Temperature 100 °C
 28.7 W/m-K
@Temperature 500 °C
Melting Point 1480 - 1530 °C
Solidus 1480 °C
Liquidus 1530 °C
Maximum Service Temperature, Air 675 °CContinuous Service
 760 °CIntermittent
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Chromium, Cr 13 %
Iron, Fe 84 %
Manganese, Mn <= 1.25 %
Molybdenum, Mo <= 0.60 %
Phosphorus, P <= 0.060 %
Silicon, Si <= 1.0 %
Sulfur, S >= 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
410 Stainless Steel
416 Stainless Steel, annealed bar
416 Stainless Steel, tempered bar
AISI 303 Cast Stainless Steel, ASTM A582
302 Stainless Steel, annealed strip

MQ416A / 13035

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.