Physical Properties | Original Value | Comments |
---|
Density | 1.01 - 1.51 g/cc |
| 0.960 - 1.17 g/cc @Temperature 270 - 330 °C |
Water Absorption | 0.0150 - 0.700 % |
Moisture Absorption at Equilibrium | 0.120 - 0.350 % |
| 0.580 - 0.580 % @Temperature 100 - 100 °C |
Water Absorption at Saturation | 0.300 - 0.400 % |
Water Vapor Transmission | 15.0 g/m²/day |
Oxygen Transmission | 65.0 - 3150 cc-mm/m²-24hr-atm |
Nitrogen Transmission | 12.0 - 630 cc-mm/m²-24hr-atm |
Carbon Dioxide Transmission | 380 - 18900 cc-mm/m²-24hr-atm |
Viscosity Number | 41.0 - 68.0 cm³/g |
Maximum Moisture Content | 0.0200 - 0.0300 |
Linear Mold Shrinkage | 0.00100 - 0.0600 cm/cm |
| 0.00700 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C |
Linear Mold Shrinkage, Transverse | 0.00260 - 0.00900 cm/cm |
| 0.00700 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C |
Melt Flow | 1.00 - 139 g/10 min |
Spiral Flow | 12.0 - 30.0 cm |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Rockwell M | 50.0 - 123 |
Hardness, Rockwell R | 72.0 - 124 |
Ball Indentation Hardness | 103 - 130 MPa |
Tensile Strength, Ultimate | 30.0 - 105 MPa |
| 23.0 - 51.0 MPa @Temperature 60.0 - 120 °C |
Tensile Strength, Yield | 40.0 - 154 MPa |
Elongation at Break | 3.00 - 233 % |
| 70.0 - 70.0 % @Temperature 60.0 - 120 °C |
Elongation at Yield | 4.00 - 118 % |
| 2.50 - 4.00 % @Temperature 60.0 - 120 °C |
Modulus of Elasticity | 1.58 - 6.00 GPa |
| 1.60 - 2.10 GPa @Temperature 60.0 - 120 °C |
Flexural Yield Strength | 27.6 - 205 MPa |
Flexural Modulus | 0.228 - 10.0 GPa |
| 1.70 - 2.20 GPa @Temperature 60.0 - 120 °C |
Flexural Strain at Break | 6.80 - 7.50 % |
Flexural Strain at Yield | 6.60 - 7.30 % |
Compressive Yield Strength | 76.0 - 86.2 MPa |
Izod Impact, Notched | 0.392 J/cm - NB |
| 0.100 - 7.48 J/cm @Temperature -40.0 - 0.000 °C |
| 2.1356 - 7.47267 J/cm @Temperature -40.0 - -30.0 °C |
| 2.1356 - 7.47267 J/cm @Thickness 3.17 - 3.20 mm |
Izod Impact, Unnotched | 0.600 - 5340 J/cm |
| 1.50 - 2.50 J/cm @Temperature -30.0 - 0.000 °C |
Izod Impact, Notched (ISO) | 6.00 - 90.0 kJ/m² |
| 10.0 - 60.0 kJ/m² @Temperature -40.0 - -20.0 °C |
| 1.20 - 150 kJ/m² @Temperature -30.0 - -20.0 °C |
| 1.20 - 150 kJ/m² @Thickness 3.00 - 3.20 mm |
Izod Impact, Unnotched (ISO) | 21000 kJ/m² |
| 20997.9 - 20997.9 kJ/m² @Temperature -30.0 - -30.0 °C |
Charpy Impact Unnotched | 4.00 J/cm² - NB |
| 2.00 J/cm² - NB @Temperature -60.0 - -20.0 °C |
| 1.60 - 1.60 J/cm² @Temperature -30.0 - -30.0 °C |
| 1.60 - 1.60 J/cm² @Thickness 3.00 - 3.00 mm |
Charpy Impact, Notched | 0.300 - 11.8 J/cm² |
| 0.600 - 5.04 J/cm² @Temperature -40.0 - -20.0 °C |
| 1.20 - 5.00 J/cm² @Temperature -30.0 - -30.0 °C |
| 1.20 - 5.00 J/cm² @Thickness 3.00 - 3.00 mm |
Gardner Impact | 36.2 - 169 J |
| >= 36.1552 J @Temperature -30.0 - -18.0 °C |
Tensile Impact Strength | 546 - 630 kJ/m² |
Dart Drop, Total Energy | 16.0 - 94.0 J |
| 11.0 - 16.0 J @Temperature -30.0 - -30.0 °C |
Falling Dart Impact | 53.8 - 1300 J |
| 75.9 - 75.9 J @Temperature -40.0 - -40.0 °C |
Puncture Energy | 45.0 - 65.0 J |
| 40.0 - 75.0 J @Temperature -30.0 - -30.0 °C |
Tensile Creep Modulus, 1 hour | 2100 - 2200 MPa |
Tensile Creep Modulus, 1000 hours | 1700 - 1900 MPa |
Taber Abrasion, mg/1000 Cycles | 10.0 |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 10200 - 1.00e+18 ohm-cm |
Surface Resistance | 100 - 4.20e+16 ohm |
Dielectric Constant | 2.70 - 3.40 |
Dielectric Strength | 11.8 - 35.0 kV/mm |
Dissipation Factor | 0.000500 - 0.0150 |
Arc Resistance | 0.000 - 120 sec |
Comparative Tracking Index | 85.0 - 600 V |
Hot Wire Ignition, HWI | 15.0 - 120 sec |
High Amp Arc Ignition, HAI | 30.0 - 120 arcs |
High Voltage Arc-Tracking Rate, HVTR | 10.0 - 150 mm/min |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 20.0 - 117 µm/m-°C |
CTE, linear, Transverse to Flow | 33.0 - 90.0 µm/m-°C |
Specific Heat Capacity | 1.26 - 2.28 J/g-°C |
Thermal Conductivity | 0.163 - 2.00 W/m-K |
Melting Point | 224 - 315 °C |
Maximum Service Temperature, Air | 116 - 150 °C |
Hot Ball Pressure Test | 90.0 - 144 °C |
Deflection Temperature at 0.46 MPa (66 psi) | 57.2 - 208 °C |
Deflection Temperature at 1.8 MPa (264 psi) | 77.8 - 187 °C |
Vicat Softening Point | 100 - 218 °C |
Minimum Service Temperature, Air | -40.0 °C |
Glass Transition Temp, Tg | 142 - 152 °C |
UL RTI, Electrical | 75.0 - 154 °C |
UL RTI, Mechanical with Impact | 75.0 - 130 °C |
UL RTI, Mechanical without Impact | 75.0 - 150 °C |
Flammability, UL94 | HB - 5VA |
Flash Point | 450 - 550 °C |
Oxygen Index | 22.0 - 40.0 % |
Glow Wire Test | 675 - 960 °C |
Ignition Temperature | 530 - 550 °C |
|
Optical Properties | Original Value | Comments |
---|
Refractive Index | 1.51 - 1.59 |
Haze | 0.100 - 100 % |
Gloss | 3.00 - 90.0 % |
Transmission, Visible | 20.0 - 93.0 % |
UV Transmittance | 88.0 % |
|
Processing Properties | Original Value | Comments |
---|
Processing Temperature | 249 - 320 °C |
Nozzle Temperature | 227 - 343 °C |
Melt Temperature | 210 - 343 °C |
Mold Temperature | 32.2 - 160 °C |
Injection Velocity | 200 mm/sec |
Drying Temperature | 70.0 - 130 °C |
Moisture Content | 0.0100 - 0.0400 % |
Dew Point | -28.9 - -17.8 °C |
Drying Air Flow Rate | 22.7 - 28.3 l/min |
Injection Pressure | 5.52 - 152 MPa |
Vent Depth | 0.00127 - 0.00762 cm |
Cushion | 0.635 cm |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.