MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Medalist® MD-50133 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Medalist MD-50133 is a clear high performance thermoplastic elastomer specifically designed for medical and healthcare applications. Medalist MD-50133 is a low hardness, low density, halogen-free grade that is suitable for extrusion or molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Processability; Good Sterilizability; Halogen Free; High Clarity; Low Density; Low Hardness; Low Specific Gravity

Uses: Medical/Healthcare Applications; Pharmaceuticals; Safety Equipment

Agency Ratings: ISO 13485

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.880 g/ccASTM D792
Melt Flow 160 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 30
@Time 15.0 sec
ASTM D2240
 33
@Time 5.00 sec
ASTM D2240
 35
@Time 1.00 sec
ASTM D2240
Tensile Strength at Break 650 psiASTM D412
Elongation at Break 680 %ASTM D412
 
Processing PropertiesOriginal ValueComments
Processing Temperature 340 - 380 °FMelt, Injection
Rear Barrel Temperature 260 - 300 °FInjection
Middle Barrel Temperature 280 - 320 °FInjection
Front Barrel Temperature 300 - 340 °FInjection
Nozzle Temperature 340 - 380 °FInjection
Zone 1 340 - 370 °FExtrusion
Zone 2 360 - 385 °FExtrusion
Zone 3 350 - 400 °FExtrusion
Zone 4 365 - 400 °FExtrusion
Zone 5 400 - 440 °FExtrusion
Die Temperature 400 - 440 °FExtrusion
Mold Temperature 70.0 - 100 °FInjection
Injection Pressure 200 - 800 psiInjection
Back Pressure 25.0 - 100 psiInjection
Cushion 0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpmExtrusion
 50 - 100 rpmInjection
 
Descriptive Properties
AppearanceClear

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-100 Thermoplastic Elastomer
Covestro Apec® 1745 Polycarbonate
Teknor Apex Medalist® MD-37063 Thermoplastic Elastomer
Teknor Apex Medalist® MD-36048 Thermoplastic Elastomer
Teknor Apex Medalist® MD-34065 Thermoplastic Elastomer

PTEKNQ0726 / 237217

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.