MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI Type S45500 Stainless Steel, hardened at 815°C (1500°F) for 30 minutes, water quenched, aged at 480°C (900°F) for 4 hours
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T S40000 Series Stainless Steel

Material Notes: Martensitic, age-hardenable, easily formable (annealed), no corrosion in fresh water, resists staining in normal air atmosphere, good resistance to pitting in 5% salt spray and 5% ferric chloride. For use in service temperatures up to 425°C.

Key Words: UNS S45500, AMS 5578, AMS 5617, AMS 5672, AMS 5860, ASTM A313 (XM-16), ASTM A564 (XM-16), ASTM A705 (XM-16), martensitic, pitting resistant, T S45518
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 472
@Temperature 23.0 - 425 °C
Converted from Rockwell C hardness.
Hardness, Knoop 522
@Temperature 23.0 - 425 °C
Converted from Rockwell C hardness.
Hardness, Rockwell C 49
@Temperature 23.0 - 425 °C
Hardness, Vickers 502
@Temperature 23.0 - 425 °C
Converted from Rockwell C hardness.
Tensile Strength, Ultimate 1240 MPa
@Temperature 425 °C
 1345 MPa
@Temperature 370 °C
 1405 MPa
@Temperature 315 °C
 1475 MPa
@Temperature 260 °C
 1690 MPa
@Temperature 23.0 °C
Tensile Strength, Yield 1145 MPa
@Strain 0.2 %,
Temperature 425 °C
 1240 MPa
@Strain 0.2 %,
Temperature 370 °C
 1295 MPa
@Strain 0.2 %,
Temperature 315 °C
 1370 MPa
@Strain 0.2 %,
Temperature 260 °C
 1635 MPa
@Strain 0.2 %,
Temperature 23.0 °C
Elongation at Break 10 %
@Temperature 260 °C
in 50 mm
 11 %
@Temperature 315 °C
in 50 mm
 11 %
@Temperature 23.0 °C
in 50 mm
 12 %
@Temperature 370 °C
in 50 mm
 14 %
@Temperature 425 °C
in 50 mm
Modulus of Elasticity 200 GPaTypical for stainless steel
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000900 ohm-cmannealed, 0.000075 Ohm-cm when annealed and aged at 510°C for 4 hours and air cooled.
 0.0000750 ohm-cm
@Temperature 23.0 °C
annealed and aged at 510°C for 4 hours and air cooled
 0.0000900 ohm-cm
@Temperature 23.0 °C
annealed
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.6 µm/m-°C
@Temperature 22.0 - 95.0 °C
 10.8 µm/m-°C
@Temperature 22.0 - 150 °C
 11.2 µm/m-°C
@Temperature 22.0 - 205 °C
 11.7 µm/m-°C
@Temperature 22.0 - 260 °C
 12.1 µm/m-°C
@Temperature 22.0 - 315 °C
Specific Heat Capacity 0.480 J/g-°CTypical value for stainless steel.
Thermal Conductivity 18.0 W/m-K
@Temperature 100 °C
 19.7 W/m-K
@Temperature 200 °C
 21.3 W/m-K
@Temperature 300 °C
 23.4 W/m-K
@Temperature 400 °C
 24.7 W/m-K
@Temperature 500 °C
Maximum Service Temperature, Air 425 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.050 %
Chromium, Cr 11.8 %
Copper, Cu 2.0 %
Iron, Fe 73 %
Manganese, Mn <= 0.50 %
Molybdenum, Mo <= 0.50 %
Nickel, Ni 8.5 %
Niobium, Nb (Columbium, Cb) 2.0 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 0.50 %
Sulfur, S <= 0.030 %
Titanium, Ti 1.1 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type S45500 Stainless Steel, hardened at 510°C (950°F) for 4 hours, air cooled
AISI Type S45500 Stainless Steel, hardened at 480°C (900°F) for 4 hours, air cooled
AISI Type S45500 Stainless Steel, annealed at 815°C (1500°F) for 30 minutes, water quenched, bar
AISI Type O1 Oil-hardening Tool Steel, oil quenched at 800°C, tempered at 425°C
AISI Type H13 Hot Work Tool Steel

MQM455S / 13852

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.