MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SABIC VALOX™ FR 771 PBT (Europe)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: VALOX 771 is a 35% mineral/glass filled, flame retardant Polybutylene Terephthalate (PBT) injection moldable grade. It has excellent chemical resistance and a UL94V0@0.75 flame rating and 5VA@2.0mm. This grade also has a CTI of 0 and is a good candidate for applications that may see electrical arcing.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.70 g/ccASTM D792
Density 1.70 g/ccISO 1183
Filler Content 35 %ASTM D229
Water Absorption 0.94 %23°C/sat; ISO 62
Moisture Absorption 0.0900 %23°C / 50% RH; ISO 62
Viscosity 140 cP
@Shear Rate 1500 1/s,
Temperature 260 °C
melt; ISO 11443
Linear Mold Shrinkage, Flow 0.0030 - 0.0060 cm/cmSABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.010 cm/cmSABIC method
Melt Flow 8.0 g/10 min
@Load 5.00 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
 16 g/10 min
@Load 5.00 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 20 g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 111ISO 2039-2
Ball Indentation Hardness 120 MPaISO 2039-1
Tensile Strength at Break 85.0 MPa5 mm/min; ISO 527
 85.0 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 85.0 MPa5 mm/min; ISO 527
 85.0 MPa5 mm/min; ASTM D638
Elongation at Break 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Elongation at Yield 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Tensile Modulus 9500 MPa5 mm/min; ASTM D638
 9700 MPa1mm/min; ISO 527
Flexural Strength 110 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
 120 MPa2 mm/min; break; ISO 178
Flexural Yield Strength 110 MPa1.3 mm/min, 50 mm span; ASTM D790
 120 MPa2 mm/min; ISO 178
Flexural Modulus 7900 MPa1.3 mm/min, 50 mm span; ASTM D790
 8400 MPa2 mm/min; ISO 178
Flexural Strain at Break 2.0 %2 mm/min; ISO 178
Izod Impact, Notched 52.0 J/mASTM D256
 51.0 J/m
@Temperature -30.0 °C
ASTM D256
 52.0 J/m
@Temperature 0.000 °C
ASTM D256
Izod Impact, Unnotched 390 J/mASTM D4812
 390 J/m
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 5.00 kJ/m²80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
 5.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 25.0 kJ/m²80*10*4; ISO 180/1U
 25.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 29.0 kJ/m²ISO 179/2C
 45.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 20.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
 29.0 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Charpy Impact, Notched 4.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 6.00 kJ/m²ISO 179/2C
 4.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
 6.00 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
Taber Abrasion, mg/1000 Cycles 55CS-17, 1 kg; SABIC method
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmASTM D257
 >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.1
@Frequency 1e+6 Hz
IEC 60250
 3.3
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 20.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 23.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
Dissipation Factor 0.0095
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.0128
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 180 - 240 secASTM D495
Comparative Tracking Index 175 VIEC 60112
 600 VIEC 60112
Hot Wire Ignition, HWI >= 120 secUL 746A
High Amp Arc Ignition, HAI >= 120 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR 0.000 - 10.0 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 22.5 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 30.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 30.1 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
CTE, linear, Transverse to Flow 59.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 95.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 135 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Hot Ball Pressure Test 125 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 215 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
 220 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 220 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 190 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 190 °C1.8 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
 203 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 190 °CRate B/50; ASTM D1525
 190 °CRate B/120; ISO 306
 190 °CRate B/50; ISO 306
 220 °CRate A/50; ISO 306
 220 °CRate A/50; ASTM D1525
UL RTI, Electrical 120 °CUL 746B
UL RTI, Mechanical with Impact 125 °CUL 746B
UL RTI, Mechanical without Impact 140 °CUL 746B
Flammability, UL94 V-2
@Thickness 0.620 mm
UL 94
 V-0
@Thickness 0.750 mm
UL 94
 5VA
@Thickness 2.00 mm
UL 94
Oxygen Index 31 %ISO 4589
Glow Wire Test 675 °C
@Thickness 2.00 mm
IEC 60695-2-13
 675 °C
@Thickness 1.00 mm
IEC 60695-2-13
 775 °C
@Thickness 3.00 mm
IEC 60695-2-13
 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Processing Temperature 40.0 - 60.0 °CHopper Temperature
Nozzle Temperature 240 - 260 °CInjection Molding
Zone 1 230 - 245 °C
Zone 2 240 - 255 °C
Zone 3 245 - 265 °C
Melt Temperature 250 - 270 °C
Mold Temperature 40.0 - 100 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 2.00 - 4.00 hourInjection Molding
Moisture Content 0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10322 / 243789

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.