MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Teknor Apex Monprene® CP-10150H Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene CP-10150H, available in NAT and colors, is a high performance thermoplastic elastomer designed for consumer product applications requiring a soft, rubber-like feel. Monprene CP-10150H is a low density, low hardness, halogen free grade that is suitable for injection molding.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Chemical Resistant; Good Colorability; Good Flexibility; Good Moldability; Good Toughness; Halogen Free; High Flow; Low Density; Low Hardness; Low Specific Gravity; Resilient; Slip; Without Fillers

Uses: Bladders; Bushings; Connectors; Consumer Applications; Flexible Grips; Grommets; Handles; Knobs; Plugs; Prototyping; Rubber Replacement; Safety Equipment; Seals

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Preliminary data. Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.885 g/ccASTM D792
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 50
@Time 5.00 sec
Injection Molded; ASTM D2240
 52
@Time 1.00 sec
Injection Molded; ASTM D2240
Tensile Strength at Break 715 psiDie C, 20 in/min; ASTM D412
Tensile Stress at Strain 195 psi
@Strain 50 %
Die C, 20 in/min; ASTM D412
 240 psi
@Strain 100 %
Die C, 20 in/min; ASTM D412
 375 psi
@Strain 300 %
Die C, 20 in/min; ASTM D412
Elongation at Break 640 %Die C, 20 in/min; ASTM D412
Tear Strength 127 pliDie C, 20 in/min; ASTM D624
Compression Set 19 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ASTM D395
 81 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ASTM D395
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 320 - 350 °F
Middle Barrel Temperature 360 - 400 °F
Front Barrel Temperature 380 - 420 °F
Nozzle Temperature 360 - 440 °F
Melt Temperature 360 - 440 °F
Mold Temperature 80.0 - 120 °F
Back Pressure 25.0 - 100 psi
Cushion 0.150 - 0.500 in
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AppearanceColors Available
 Natural Color
 Translucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ0761 / 237252

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.