MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Magnesium ZH62A-T5, Cast
Categories: Metal; Nonferrous Metal; Magnesium Alloy

Material Notes:

Key Words: UNS M16620; Mg
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.86 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 70500 kg load, 10 mm ball
Hardness, Knoop 93Estimated from Brinell
Hardness, Vickers 80Estimated from Brinell
Tensile Strength, Ultimate 240 MPa
 320 MPa
@Temperature -196 °C
 330 MPa
@Temperature -78.0 °C
 69.0 MPa
@Temperature 315 °C,
Time 601 sec
tested at elevated temperature
 195 MPa
@Temperature 150 °C,
Time 601 sec
tested at elevated temperature
Tensile Strength, Yield 200 MPa
@Temperature -78.0 °C
 235 MPa
@Temperature -196 °C
 170 MPa
@Strain 0.2 %
Elongation at Break 4.0 %in 50 mm
 1.0 %
@Temperature -196 °C
 2.7 %
@Temperature -78.0 °C
Creep Strength 17.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.2% total extension
Modulus of Elasticity 38.0 GPa
@Temperature 315 °C
 40.0 GPa
@Temperature 205 °C
Tensile Modulus 45.0 GPa
Compressive Yield Strength 170 MPaat 0.2% offset
Ultimate Bearing Strength 495 MPa
Bearing Yield Strength 340 MPa
Poissons Ratio 0.30
Machinability 100 %Relative Rating, 100=Best
Shear Modulus 17.0 GPa
Shear Strength 165 MPa
Charpy Impact 1.02 JV-notch
 1.02 J
@Temperature -78.0 °C
Notched
 1.02 J
@Temperature -196 °C
Notched
Charpy Impact, Unnotched 8.56 J
@Temperature -196 °C
 15.02 J
@Temperature 24.0 °C
 18.99 J
@Temperature -78.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000650 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 373 J/g
CTE, linear 27.0 µm/m-°C
@Temperature 20.0 - 200 °C
Estimated from similar Mg alloys
 27.1 µm/m-°C
@Temperature 0.000 - 100 °C
Specific Heat Capacity 0.960 J/g-°C
Thermal Conductivity 110 W/m-K
Melting Point 520 - 630 °C
Solidus 520 °C
Liquidus 630 °C
 
Processing PropertiesOriginal ValueComments
Casting Temperature 750 - 820 °CSand Casting
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu <= 0.10 %
Magnesium, Mg 92 %As Remainder
Nickel, Ni <= 0.010 %
Thorium, Th 1.4 - 2.2 %
Zinc, Zn 5.2 - 6.2 %
Zirconium, Zr 0.50 - 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Magnesium ZC63-T6
Magnesium ZE41A-T5, Cast
Magnesium ZK31-T5, Forgings
Magnesium ZK40A-T5, Extruded
Magnesium ZK51A-T5, Cast

MMZH62 / 12474

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.