System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Envalior Durethan® BM 25 FN20 DUS013 000000 Nylon 6 (PA6), 25% Mineral Filled, Dry
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
;
Nylon 6, 30% Mineral Filled
Material Notes:
PA 6, 25% mineral, injection molding, halogen free flame retardant, optimized for laser marking (1064nm)
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.425
g/cc
ISO 1183
Water Absorption at Saturation
6.7 %
IOS 62
Linear Mold Shrinkage, Flow
0.0090
cm/cm
60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0090
cm/cm
60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
Mechanical Properties
Original Value
Comments
Ball Indentation Hardness
178
MPa
ISO 2093-1
Tensile Strength at Break
80.0
MPa
5 mm/min; ISO 527-1,-2
Tensile Strength, Yield
80.0
MPa
50 mm/min; ISO 527-1,-2
Elongation at Break
3.0 %
5 mm/min; ISO 527-1,-2
Elongation at Yield
3.0 %
50 mm/min; ISO 527-1,-2
Tensile Modulus
5700
MPa
1 mm/min; ISO 527-1,-2
Flexural Strength
130
MPa
2 mm/min; ISO 178-A
Flexural Yield Strength
130
MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus
5500
MPa
2 mm/min; ISO 178-A
Flexural Strain at Break
3.3 %
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
<=
10.0
kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO)
30.0
kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched
38.0
kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Electrical Properties
Original Value
Comments
Comparative Tracking Index
1.0
V
Solution A; UL 746A
450
V
Solution A; IEC 60112
Hot Wire Ignition, HWI
7.0
-
15
sec
UL 746A
15
-
30
sec
UL 746A
30
-
60
sec
UL 746A
High Amp Arc Ignition, HAI
>=
120
arcs
PLC 0; UL 746A
>=
120
arcs
PLC 0; UL 746A
>=
120
arcs
PLC 0; UL 746A
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
60.0
µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow
70.0
µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point
220
°C
10°C/min; ISO 11357-1,-3
Maximum Service Temperature, Air
205
°C
IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi)
195
°C
ISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi)
90.0
°C
ISO 75-1,-2
Vicat Softening Point
206
°C
@Load 5.10 kg
120°C/h; ISO 306
Flammability, UL94
V-2
@Thickness 1.50 mm
V-2
@Thickness 0.750 mm
V-2
@Thickness 3.00 mm
Glow Wire Ignition Temperature
725
°C
@Thickness 0.750 mm
IEC 60695-2-13
725
°C
@Thickness 1.50 mm
IEC 60695-2-13
725
°C
@Thickness 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index
960
°C
@Thickness 0.800 mm
IEC 60695-2-12
960
°C
@Thickness 1.50 mm
IEC 60695-2-12
960
°C
@Thickness 3.00 mm
IEC 60695-2-12
Shrinkage, MD
0.20 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction; 60x60x2; ISO 294-4
Shrinkage, TD
0.20 %
@Treatment Temp. 120 °C,
Time 14400 sec
60x60x2; ISO 294-4
Processing Properties
Original Value
Comments
Melt Temperature
260
°C
injection molding
250
-
270
°C
Mold Temperature
80.0
°C
injection molding
80.0
-
100
°C
Drying Temperature
80.0
°C
Dry Time
2.00
-
6.00
hour
Moisture Content
0.030 - 0.070 %
Karl Fischer
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Nylon 6, Nucleated
Domo TECHNYL® 1015CR PA6, DRY
PLANW9450 / 208283
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.