MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay Chemicals Hydrochloric Acid 31% - Technical Grade (2 wt% - 10 wt% Concentration)
Categories: Fluid

Material Notes: Hydrochloric acid, also known as muriatic acid, is a colorless to yellow liquid, with a pungent odor. Hydrochloric acid is a strong acid used as chemical reagent, pH-regulating, ion exchanger regenerating, pickling or cleaning agent.

EINECS: 231-595-7/CAS: 7647-01-0/UN: 1789

Information provided by Solvay

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.9639 g/cc
@Temperature 100 °C
Concentration 0.01 kg HCl/kg
 0.9688 g/cc
@Temperature 100 °C
Concentration 0.02 kg HCl/kg
 0.9791 g/cc
@Temperature 100 °C
Concentration 0.04 kg HCl/kg
 0.9892 g/cc
@Temperature 100 °C
Concentration 0.06 kg HCl/kg
 0.997 g/cc
@Temperature 40.0 °C
Concentration 0.01 kg HCl/kg
 0.9992 g/cc
@Temperature 100 °C
Concentration 0.08 kg HCl/kg
 1.0019 g/cc
@Temperature 40.0 °C
Concentration 0.02 kg HCl/kg
 1.0048 g/cc
@Temperature -5.00 °C
Concentration 0.01 kg HCl/kg
 1.009 g/cc
@Temperature 100 °C
Concentration 0.10 kg HCl/kg
 1.0104 g/cc
@Temperature -5.00 °C
Concentration 0.02 kg HCl/kg
 1.0116 g/cc
@Temperature 40.0 °C
Concentration 0.04 kg HCl/kg
 1.0211 g/cc
@Temperature 40.0 °C
Concentration 0.06 kg HCl/kg
 1.0213 g/cc
@Temperature -5.00 °C
Concentration 0.04 kg HCl/kg
 1.0305 g/cc
@Temperature 40.0 °C
Concentration 0.08 kg HCl/kg
 1.0321 g/cc
@Temperature -5.00 °C
Concentration 0.06 kg HCl/kg
 1.04 g/cc
@Temperature 40.0 °C
Concentration 0.10 kg HCl/kg
 1.0428 g/cc
@Temperature -5.00 °C
Concentration 0.08 kg HCl/kg
 1.0536 g/cc
@Temperature -5.00 °C
Concentration 0.10 kg HCl/kg
Viscosity 0.30 cP
@Temperature 100 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 0.31 cP
@Temperature 100 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 0.38 cP
@Temperature 80.0 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 0.41 cP
@Temperature 80.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 0.51 cP
@Temperature 60.0 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 0.56 cP
@Temperature 60.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 0.72 cP
@Temperature 40.0 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 0.79 cP
@Temperature 40.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 1.1 cP
@Temperature 20.0 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 1.19 cP
@Temperature 20.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 1.4 cP
@Temperature 10.0 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 1.5 cP
@Temperature 10.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 1.84 cP
@Temperature 0.000 °C
Dynamic, Concentration 0.05 kg FeCl3/kg
 1.94 cP
@Temperature 0.000 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
 2.58 cP
@Temperature -10.0 °C
Dynamic, Concentration 0.10 kg FeCl3/kg
Molecular Weight 36.47 g/molHCl
Vapor Pressure 0.00200 bar
@Temperature -10.0 °C
Concentration 0.10 kg HCl/kg
 0.00500 bar
@Temperature 0.000 °C
Concentration 0.10 kg HCl/kg
 0.00600 bar
@Temperature 0.000 °C
Concentration 0.05 kg HCl/kg
 0.0110 bar
@Temperature 10.0 °C
Concentration 0.10 kg HCl/kg
 0.0120 bar
@Temperature 10.0 °C
Concentration 0.05 kg HCl/kg
 0.0210 bar
@Temperature 20.0 °C
Concentration 0.10 kg HCl/kg
 0.0220 bar
@Temperature 20.0 °C
Concentration 0.05 kg HCl/kg
 0.0650 bar
@Temperature 40.0 °C
Concentration 0.10 kg HCl/kg
 0.0700 bar
@Temperature 40.0 °C
Concentration 0.05 kg HCl/kg
 0.170 bar
@Temperature 60.0 °C
Concentration 0.10 kg HCl/kg
 0.190 bar
@Temperature 60.0 °C
Concentration 0.05 kg HCl/kg
 0.410 bar
@Temperature 80.0 °C
Concentration 0.10 kg HCl/kg
 0.450 bar
@Temperature 80.0 °C
Concentration 0.05 kg HCl/kg
 0.890 bar
@Temperature 100 °C
Concentration 0.10 kg HCl/kg
 0.970 bar
@Temperature 100 °C
Concentration 0.05 kg HCl/kg
Surface Tension 0.061 dynes/cm
@Temperature 100 °C
Concentration 0.05 HCl/kg
 0.063 dynes/cm
@Temperature 100 °C
Concentration 0.10 HCl/kg
 0.064 dynes/cm
@Temperature 80.0 °C
Concentration 0.05 HCl/kg
 0.065 dynes/cm
@Temperature 80.0 °C
Concentration 0.10 HCl/kg
 0.067 dynes/cm
@Temperature 60.0 °C
Concentration 0.05 HCl/kg
 0.068 dynes/cm
@Temperature 60.0 °C
Concentration 0.10 HCl/kg
 0.070 dynes/cm
@Temperature 40.0 °C
Concentration 0.05 HCl/kg
 0.070 dynes/cm
@Temperature 40.0 °C
Concentration 0.10 HCl/kg
 0.072 dynes/cm
@Temperature 20.0 °C
Concentration 0.10 HCl/kg
 0.073 dynes/cm
@Temperature 10.0 °C
Concentration 0.10 HCl/kg
 0.073 dynes/cm
@Temperature 20.0 °C
Concentration 0.05 HCl/kg
 0.074 dynes/cm
@Temperature 0.000 °C
Concentration 0.10 HCl/kg
 0.074 dynes/cm
@Temperature 10.0 °C
Concentration 0.05 HCl/kg
 0.075 dynes/cm
@Temperature -10.0 °C
Concentration 0.10 HCl/kg
 0.075 dynes/cm
@Temperature 0.000 °C
Concentration 0.05 HCl/kg
 0.076 dynes/cm
@Temperature -10.0 °C
Concentration 0.05 HCl/kg
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 3.30 J/g-°C
@Temperature -10.0 °C
Concentration 0.10 kg HCl/kg
 3.40 J/g-°C
@Temperature 0.000 °C
Concentration 0.10 kg HCl/kg
 3.40 J/g-°C
@Temperature 10.0 °C
Concentration 0.10 kg HCl/kg
 3.40 J/g-°C
@Temperature 20.0 °C
Concentration 0.10 kg HCl/kg
 3.50 J/g-°C
@Temperature 40.0 °C
Concentration 0.10 kg HCl/kg
 3.60 J/g-°C
@Temperature 60.0 °C
Concentration 0.10 kg HCl/kg
 3.60 J/g-°C
@Temperature 80.0 °C
Concentration 0.10 kg HCl/kg
 3.70 J/g-°C
@Temperature 100 °C
Concentration 0.10 kg HCl/kg
 3.80 J/g-°C
@Temperature 20.0 °C
Concentration 0.05 kg HCl/kg
 3.80 J/g-°C
@Temperature 10.0 °C
Concentration 0.05 kg HCl/kg
 3.80 J/g-°C
@Temperature 0.000 °C
Concentration 0.05 kg HCl/kg
 3.90 J/g-°C
@Temperature 100 °C
Concentration 0.05 kg HCl/kg
 3.90 J/g-°C
@Temperature 40.0 °C
Concentration 0.05 kg HCl/kg
 3.90 J/g-°C
@Temperature 80.0 °C
Concentration 0.05 kg HCl/kg
 3.90 J/g-°C
@Temperature 60.0 °C
Concentration 0.05 kg HCl/kg
Thermal Conductivity 0.520 W/m-K
@Temperature -10.0 °C
Concentration 0.10 kg HCl/kg
 0.530 W/m-K
@Temperature 0.000 °C
Concentration 0.10 kg HCl/kg
 0.550 W/m-K
@Temperature 0.000 °C
Concentration 0.05 kg HCl/kg
 0.550 W/m-K
@Temperature 10.0 °C
Concentration 0.10 kg HCl/kg
 0.560 W/m-K
@Temperature 20.0 °C
Concentration 0.10 kg HCl/kg
 0.560 W/m-K
@Temperature 10.0 °C
Concentration 0.05 kg HCl/kg
 0.570 W/m-K
@Temperature 20.0 °C
Concentration 0.05 kg HCl/kg
 0.580 W/m-K
@Temperature 40.0 °C
Concentration 0.10 kg HCl/kg
 0.600 W/m-K
@Temperature 60.0 °C
Concentration 0.10 kg HCl/kg
 0.600 W/m-K
@Temperature 40.0 °C
Concentration 0.05 kg HCl/kg
 0.620 W/m-K
@Temperature 80.0 °C
Concentration 0.10 kg HCl/kg
 0.620 W/m-K
@Temperature 60.0 °C
Concentration 0.05 kg HCl/kg
 0.640 W/m-K
@Temperature 80.0 °C
Concentration 0.05 kg HCl/kg
 0.640 W/m-K
@Temperature 100 °C
Concentration 0.10 kg HCl/kg
 0.670 W/m-K
@Temperature 100 °C
Concentration 0.05 kg HCl/kg
Melting Point -15.0 °CConcentration 0.10 kg HCl/kg
 -6.00 °CConcentration 0.05 kg HCl/kg
Boiling Point 101 °C
@Pressure 0.101 MPa
Concentration 0.05 kg HCl/kg
 103 °C
@Pressure 0.101 MPa
Concentration 0.10 kg HCl/kg
 
Descriptive Properties
Composition<2 mg/kgHeavy Metals, ISO 11885
 <20 mg/kgSulfate (SO4), IOS 2762
 <3 mg/kgIron (Fe), ISO 6685
 <5 mg/kgFluoride (F), IOS 10359-1
 300-320 g/kgHydrochloric Acid (HCl), ISO 904

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Epoxy Technology EPO-TEK® T7109-17 Thermally Conductive Epoxy
Parson Adhesives PARFIX® 3401 Cyanoacrylate Adhesive
Epoxy Technology EPO-TEK® T7110 Thermally Conductive, Room-Temperature Cure Epoxy
3M Novec™ 774 Engineered Fluid

WSOLV137 / 147786

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.