MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Manifattura Cattaneo VESPEL® SP21 Polyimide
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: Manifattura Cattaneo products are available in semi-finished forms such as bars, profiles, sheets and plates.

Information provided by Manifattura Cattaneo s.p.a.

Key Words: DuPont™ VESPEL®
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.51 g/ccASTM D792
Moisture Absorption at Equilibrium 0.80 - 1.1 %
@Temperature 23.0 °C
50% RH; ASTM D570
Water Absorption at Saturation 0.57 %ASTM D570
Deformation 0.70 %
@Time 86400 sec,
Pressure 100 MPa
ASTM D621
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 66.0 MPaASTM D638
Elongation at Break 4.5 %ASTM D638
Tensile Modulus 2620 MPaASTM D638
Flexural Strength 110 MPaASTM D790
Compressive Yield Strength 29.0 MPa
@Strain 1 %,
Time 3.60e+6 sec
ASTM D695
Compressive Modulus 2895 MPaASTM D695
Poissons Ratio 0.41
Izod Impact, Notched (ISO) 0.0430 kJ/m²ASTM D256
Izod Impact, Unnotched (ISO) 0.320 kJ/m²ASTM D256
Coefficient of Friction, Dynamic 0.24on polished steel; MPC Test
Coefficient of Friction, Static 0.30on polished steel; MPC Test
K Factor (Wear Factor) 0.43µm/s. PV = 0.1 MPa-m/s; max P = 30 MPa; MPC Test
Limiting Pressure Velocity 12.0 MPa-m/secwithout lubrication; MPC Test
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+14 ohm-cmASTM D257
Dielectric Constant 13.41
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 9.48 kV/mm
@Thickness 2.00 mm
ASTM D149
Dielectric Loss Index 0.0106
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 49.0 µm/m-°C
@Temperature 23.0 - 100 °C
Thermal Conductivity 0.870 W/m-KASTM D177
Maximum Service Temperature, Air 395 °C
Deflection Temperature at 1.8 MPa (264 psi) 360 °CASTM D648-45
Flammability, UL94 V-0
Oxygen Index 49 %ASTM D2863
 
Compliance PropertiesOriginal ValueComments
FDA No
 
Descriptive Properties
ColorDark Gray
UV ResistanceN

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® SCP-5050 Polyimide
Arkema KYNAR® 740 Polyvinylidene Fluoride Homopolymer - Injection Molding and Extrusion
Manifattura Cattaneo VESPEL® SP1 Polyimide
Manifattura Cattaneo VESPEL® SP22 Polyimide
ALM PA 605-A Filled Nylon 12 Prototyping Polymer

PMANIF917 / 156197

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.