MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC NORYL GTX™ Resin NX0031 Polyphenylene Ether + PA (PPE+Nylon)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Polyphenylene Ether/PPO

Material Notes: NORYL GTX™ NX0031 resin is a non-reinforced alloy of PPE/PA. This conductive, injection moldable grade exhibits high heat resistance, excellent chemical resistance, and high impact resistance. NORYL NX0031 resin was designed for electrostatic painting and powder coating without the need for a conductive primer. This material can also be solvent painted and is an excellent for candidate for exterior, painted applications such as trim and fairings for outdoor vehicles, motorcycle, heavy truck, bus, personal watercraft, and marine. It is available only in black.

Features: Hydrolytic Stability,Chemical Resistance,Low Creep Sensitivity,Good Stiffness,Low Warpage,High Impact Resistance,Heat Stabilized,Good Processability,Conductive,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.09 g/ccASTM D792
Density 1.09 g/ccISO 1183
Moisture Absorption 0.0700 %Injection Molding
 1.20 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 4.2 %ISO 62-1
Viscosity 8.0 cP
@Load 5.00 kg,
Temperature 280 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.013 - 0.016 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 8.0 g/10 min
@Load 5.00 kg,
Temperature 280 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 48.0 MPa50 mm/min; ASTM D638
 48.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 50.0 MPa50 mm/min; ISO 527
 52.0 MPa50 mm/min; ASTM D638
Elongation at Break 30 %50 mm/min; ISO 527
 34 %50 mm/min; ASTM D638
Elongation at Yield 4.0 %50 mm/min; ISO 527
 5.0 %50 mm/min; ASTM D638
Tensile Modulus 2000 MPa1 mm/min; ISO 527
 2250 MPa5 mm/min; ASTM D638
Flexural Strength 75.0 MPayield, 2 mm/min; ISO 178
 79.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 1900 MPa2 mm/min; ISO 178
 2100 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 224 JASTM D256
 117 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 20.0 kJ/m²80*10*4; ISO 180/1A
 10.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 18.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 10.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 42.0 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 100 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 100 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 90.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
 100 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 176 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 136 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 175 °CRate B/50; ASTM D1525
 175 °CRate B/50; ISO 306
 180 °CRate B/120; ISO 306
Flammability, UL94 HB
@Thickness >=1.50 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 270 - 295 °C
Zone 2 260 - 295 °C
Zone 3 265 - 295 °C
Melt Temperature 270 - 295 °CInjection Molding
Mold Temperature 65.0 - 95.0 °C
Drying Temperature 95.0 - 105 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 8.00 hourCumulative; Injection Molding
Moisture Content 0.020 %minimum
Back Pressure 0.300 - 1.40 MPa
Shot Size 30 - 50 %
Vent Depth 0.00130 - 0.00380 cm
Screw Speed 20 - 100 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82205 / 290152

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.