MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Celanese Celstran® PA6-GF50-01 Nylon 6, 50% Glass Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 50% Glass Fiber Filled

Material Notes: 50% long strand fiber glass reinforced nylon 6 Natural

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.56 g/ccASTM D792
Density 1.56 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.00050 - 0.0010 cm/cmASTM D955
Linear Mold Shrinkage, Transverse 0.0020 - 0.0030 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 245 MPa5mm/min; ISO 527-2/1A
 39400 psiASTM D638
 17900 psi
@Temperature 121 °C
ASTM D638
 46650 psi
@Temperature -40.0 °C
ASTM D638
Elongation at Break 2.02 %5mm/min; ISO 527-2/1A
 2.2 %ASTM D638
 2.3 %
@Temperature 121 °C
ASTM D638
 2.6 %
@Temperature 4.44 °C
ASTM D638
Tensile Modulus 16000 MPa50mm/min; ISO 527-2/1A
 2.55e+6 psiASTM D638
 1.31e+6 psi
@Temperature 121 °C
ASTM D638
 2.32e+6 psi
@Temperature -40.0 °C
ASTM D638
Flexural Strength 390 MPaISO 178
 57000 psiASTM D790
 25600 psi
@Temperature 121 °C
ASTM D790
 62810 psi
@Temperature -40.0 °C
ASTM D790
Flexural Modulus 14700 MPaISO 178
 2.13e+6 psiASTM D790
 1.18e+6 psi
@Temperature 121 °C
ASTM D790
 2.24e+6 psi
@Temperature -40.0 °C
ASTM D790
Izod Impact, Notched 9.30 ft-lb/inASTM D256
 8.90 ft-lb/in
@Temperature -40.0 °C
ASTM D256
 11.2 ft-lb/in
@Temperature 121 °C
ASTM D256
Charpy Impact, Notched 39.0 kJ/m²ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 215 °CISO 75-1, -2
 415 °FASTM D648
 
Processing PropertiesOriginal ValueComments
Processing Temperature 80.0 - 100 °Ccavity
Feed Temperature 20.0 - 50.0 °C
Zone 1 265 - 275 °C
Zone 2 270 - 275 °C
Zone 3 275 - 280 °C
Zone 4 275 - 280 °C
Die Temperature 275 - 280 °C
Melt Temperature 270 - 280 °C
Drying Temperature 70.0 - 80.0 °C
Dry Time 2.00 - 4.00 hour
Moisture Content <= 0.18 %
 
Descriptive Properties
Injection moldingYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zytel® 73G50HSLA BK416 PA6-GF50
LG Chemical LUMID SG2600B PA6+GF60%, General purpose, Good Surface
LG Chemical LUMID GP2500A(W) PA6+GF50%, General Purpose
Kolon KOPA® KN133G50 G/F Reinforced Nylon 6
Grupo Repol Dinalon® B1S25 G50 50% Glass Fiber Reinforced Nylon 6

PHCQ184 / 178639

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.