MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Oxygen-free Electronic Copper (OFE), UNS C10100, OS025 temper, flat products and tubing
Categories: Metal; Nonferrous Metal; Copper Alloy; Wrought Copper

Material Notes: Test specimens: flat product, 1 mm thick; tubing, 25 mm (1 in) OD, 1.65 mm (0.065 in) wall thickness.

Applications: busbars, bus conductors, waveguides, hollow conductors, lead-in wires and anodes for vacuum tubes, vacuum seals, transistor components, glass-to-metal seals, coaxial cables, klystrons, microwave tubes, and rectifiers.

Processing: Excellent hot and cold workability; good forgeability. Fabricated by bending, coining, coppersmithing, drawing and upsetting, hot forging and pressing, knurling, roll threading, shearing, spinning, swaging, and stamping.

Corrosion Resistance: Good to excellent. Susceptible to galvanic corrosion when coupled with iron, aluminum, magnesium, lead, tin, and zinc. Good resistance to atmospheric, brackish water, sea water, and non-oxidizing acid corrosion, but avoid heating in oxidizing atmospheres or exposing to oxidizing acids, moist halogens, sulfides, ammonia, or solutions with ammonium ions.

UNS C10100 - ASTM B48, B133, B152, B187, B272, B432, F68; 101A (Australia); C110 (UK); CDA 101 OFE; ISO Cu-OFE; JIS C1011 H3510 (Japan)

Key Words: ISO Cu-OFE, CEN CW009A, oxygen-free high conductivity copper (OFHC), CDA 101 OFE, ASTM B48, B133, B152, B187, B272, B432, F68, AS 101A 1567 (Australia), Cu/cl NF A53301, JIS C1011 H3510, flat products, plates, sheets, strips
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.94 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell F 45
Tensile Strength, Ultimate 235 MPa
Tensile Strength, Yield 76.0 MPa
@Strain 0.5 %
Elongation at Break 45 %in 50 mm (2 in)
Creep Strength 0.700 MPa
@Temperature 260 °C
Creep rate of 10-6%/h
 3.00 MPa
@Temperature 205 °C
Creep rate of 10-6%/h
 3.00 MPa
@Temperature 260 °C
Creep rate of 10-5%/h
 10.0 MPa
@Temperature 205 °C
Creep rate of 10-5%/h
 11.0 MPa
@Temperature 150 °C
Creep rate of 10-6%/h
 12.0 MPa
@Temperature 260 °C
Creep rate of 10-4%/h
 25.0 MPa
@Temperature 150 °C
Creep rate of 10-5%/h
 33.0 MPa
@Temperature 205 °C
Creep rate of 10-4%/h
 55.0 MPa
@Temperature 150 °C
Creep rate of 10-4%/h
 110 MPa
@Temperature 150 °C
Creep rate of 10-3%/h
 125 MPa
@Temperature 120 °C
Creep rate of 10-3%/h
 130 MPa
@Temperature 150 °C
Creep rate of 10-2%/h
 150 MPa
@Temperature 120 °C
Creep rate of 10-2%/h
 150 MPa
@Temperature 150 °C
Creep rate of 10-1%/h
 165 MPa
@Temperature 120 °C
Creep rate of 10-1%/h
 170 MPa
@Temperature 43.0 °C
Creep rate of 10-3%/h
 185 MPa
@Temperature 43.0 °C
Creep rate of 10-2%/h
 200 MPa
@Temperature 43.0 °C
Creep rate of 10-1%/h
Rupture Strength 106 MPa
@Temperature 200 °C,
Time 3.60e+6 sec
 130 MPa
@Temperature 200 °C,
Time 360000 sec
 147 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
 161 MPa
@Temperature 150 °C,
Time 360000 sec
Modulus of Elasticity 115 GPa
Poissons Ratio 0.31
Fatigue Strength 76.0 MPa
@Thickness 1.00 mm,
# of Cycles 1.00e+9
flat
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %UNS C37700 (forging brass) = 100%
Shear Modulus 44.0 GPa
Shear Strength 160 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000171 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 100 °C
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.385 J/g-°C
@Temperature 20.0 °C
Thermal Conductivity 391 W/m-K
@Temperature 20.0 °C
Melting Point 1083 °C
Annealing Point >= 700 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 375 - 650 °C
Hot-Working Temperature 750 - 875 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu >= 99.99 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Oxygen-free Electronic Copper (OFE), UNS C10100, H04 Temper, flat products
Oxygen-free Electronic Copper (OFE), UNS C10100, OS050 temper, flat products, rod, tubing, and shapes
Oxygen-free Electronic Copper (OFE), UNS C10100, H00 Temper, flat products
Oxygen-free Electronic Copper (OFE), UNS C10100, H01 Temper, flat products
Oxygen-free Electronic Copper (OFE), UNS C10100, H02 Temper, flat products

MC10100d1 / 10373

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.