MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Trinseo Magnum™ 345 ABS  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ABS resin are available in a wide range of melt flow rates, impact strength and heat resistance for both high and low gloss applications manufactured by injection molding, sheet or profile extrusion and thermoforming.

MAGNUM ABS resins offer a wide range of processability and impact resistance for low gloss injection molding applications. Combined with heat resistance and tensile and flexural strength, MAGNUM ABS resins are used in a wide variety of injection molding applications.

MAGNUM 345 ABS resin is the easiest processing low gloss, low impact strength injection molding resin. With a high melt flow rate of 12 g/10 min., it is often selected for hard to fill molds or long flow lengths.

Data provided by Dow Chemical.

This product line was spun off from Dow Chemical to Styron in 2010.

Key Words: Poly(Acrylonitrile Butadiene Styrene)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccASTM Data
Linear Mold Shrinkage 0.0055 cm/cm
Melt Flow 15 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM Data
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 37.9 MPaASTM Data
Elongation at Break 110 %ASTM Data
Tensile Modulus 2.08 GPaASTM Data
Izod Impact, Notched 1.33 J/cmASTM Data
Instrumented Impact Total Energy 35.0 J
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °CUnannealed; ASTM Data
Deflection Temperature at 1.8 MPa (264 psi) 77.0 °CUnannealed; ASTM Data
Vicat Softening Point 103 °C
Flammability, UL94 HB
@Thickness 1.47 mm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PZZDW084 / 34315

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.