MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
North American Loblolly Pine Wood
Categories: Wood and Natural Products; Wood; Softwood

Material Notes: Data is based on small, clear, air-dried samples unless specified.

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Pinus Taeda; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.500 g/ccOven Dry Weight/Unseasoned Volume
 54.0 lb/ft³Unseasoned*
Cell Length 3.60 mmMature Wood
 
Mechanical PropertiesOriginal ValueComments
Hardness, Wood Indentation 1800 NEnd. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 2000 NSide. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 3100 NSide
Tensile Strength, Ultimate 3.20 MPaPerpendicular to Grain
 280 psiPerpendicular to Grain*
Modulus of Rupture 0.0880 GPaStatic Bending
 7.50 ksiStatic Bending*
Flexural Yield Strength 4400 psiFiber Stress at Elastic Limit; Static Bending*
Flexural Modulus 12.42 GPaStatic Bending
 1380 ksiStatic Bending*
Compressive Strength 6.80 MPaPerpendicular to Grain
 49.0 MPaParallel to Grain
 550 psiPerpendicular to Grain*
 2870 psiParallel to Grain*
 3580 psiMax Crushing Strength Parallel to Grain*
Poissons Ratio 0.292µLT, 12% Moisture Content
 0.328µLR, 12% Moisture Content
 0.362µTR, 12% Moisture Content
 0.382µRT, 12% Moisture Content
Shear Strength 9.40 MPaOrientation Unknown
 900 psiParallel to Grain*
Impact 3.1in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 9500psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.810 in-lb/in³Static Bending*
Work to Maximum Load 8.00 in-lb/in³Static Bending*
Toughness 18.1 JRadial
 29.5 JTangential
 
Thermal PropertiesOriginal ValueComments
Thermal Conductivity 0.860 BTU-in/hr-ft²-°FOven Dry
 1.00 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 4.8 %Radial; Green to Zero Moisture
 7.4 %Tangential; Green to Zero Moisture
 12.3 %Volumetric; Green to Zero Moisture

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
American Pine Wood
Northern White Pine Wood
Southern Pine Wood
American Eastern White Pine Wood
American Longleaf Pine Wood

PTSA600 / 71267

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.