MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Envalior Durethan® BM 25 FN20 700350 Nylon 6 (PA6), 25% Mineral Filled, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Mineral Filled

Material Notes: PA 6, 25% mineral, injection molding, halogen free flame retardant

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.700 g/ccISO 60
Density 1.38 g/ccISO 1183
Water Absorption at Saturation 6.7 %IOS 62
Linear Mold Shrinkage, Flow 0.0090 cm/cm60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm60x60x2; 280 °C / MT 80°C; 600 bar; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 178 MPaISO 2093-1
Tensile Strength at Break 80.0 MPa5 mm/min; ISO 527-1,-2
Tensile Strength, Yield 80.0 MPa50 mm/min; ISO 527-1,-2
Elongation at Break 3.0 %5 mm/min; ISO 527-1,-2
Elongation at Yield 3.0 %50 mm/min; ISO 527-1,-2
Tensile Modulus 5700 MPa1 mm/min; ISO 527-1,-2
Flexural Strength 135 MPa2 mm/min; ISO 178-A
Flexural Yield Strength 130 MPa
@Strain 3.5 %
2 mm/min; ISO 178-A
Flexural Modulus 5500 MPa2 mm/min; ISO 178-A
Flexural Strain at Break 3.5 %2 mm/min; ISO 178-A
Izod Impact, Notched (ISO) <= 10.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO) 30.0 kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched 38.0 kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 1.0 VSolution A; UL 746A
 450 VSolution A; IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 secUL 746A
 15 - 30 secUL 746A
 30 - 60 secUL 746A
High Amp Arc Ignition, HAI >= 120 arcsPLC 0; UL 746A
 >= 120 arcsPLC 0; UL 746A
 >= 120 arcsPLC 0; UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 60.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1,-2
Melting Point 220 °C10°C/min; ISO 11357-1,-3
Maximum Service Temperature, Air 205 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 195 °CISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °CISO 75-1,-2
Vicat Softening Point 205 °C
@Load 5.10 kg
50°C/h; ISO 306
 206 °C
@Load 5.10 kg
120°C/h; ISO 306
Flammability, UL94 V-2
@Thickness 1.50 mm
 V-2
@Thickness 0.750 mm
 V-2
@Thickness 3.00 mm
Glow Wire Ignition Temperature 725 °C
@Thickness 0.750 mm
IEC 60695-2-13
 725 °C
@Thickness 1.50 mm
IEC 60695-2-13
 725 °C
@Thickness 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.800 mm
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
Shrinkage, MD 0.20 %
@Treatment Temp. 120 °C,
Time 14400 sec
Post-Shrinkage Flow Direction; 60x60x2; ISO 294-4
Shrinkage, TD 0.20 %
@Treatment Temp. 120 °C,
Time 14400 sec
60x60x2; ISO 294-4
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °Cinjection molding
 250 - 270 °C
Mold Temperature 80.0 °Cinjection molding
 80.0 - 100 °C
Drying Temperature 80.0 °C
Dry Time 2.00 - 6.00 hour
Moisture Content 0.030 - 0.070 %Karl Fischer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PLANW9448 / 208281

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.