MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Alclad Aluminum 2014-T4, T451
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Used in applications requiring high strength/hardness, including elevated temperature uses. Specific applications include heavy duty forgings, plate, and extrusions for aerospace fittings, wheels, tanks, and major structural components, heavy duty automotive frame and suspension componentry. 2014 exhibits poor corrosion resistance for an aluminum alloy so the clad version is used when necessary.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition for AA 2014 (not Alclad 2014 specifically).
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A82014; Alclad 2014-T4, T451; Alclad 2014-T4, T451; Al2014-T4
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.80 g/ccFor AA2014 (Not Alclad)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 61.0 ksiAA; Typical
 >= 370 MPa
@Thickness 0.508 - 0.610 mm
Coiled sheet
 >= 370 MPa
@Thickness 0.508 - 0.610 mm
Sheet and plate
 >= 380 MPa
@Thickness 0.635 - 0.991 mm
Coiled sheet
 >= 380 MPa
@Thickness 0.635 - 0.991 mm
Sheet and plate
 >= 395 MPa
@Thickness 1.02 - 6.32 mm
Coiled sheet
 >= 395 MPa
@Thickness 6.35 - 12.7 mm
Plate; T451
 >= 395 MPa
@Thickness 50.83 - 76.2 mm
Plate; T451
 >= 395 MPa
@Thickness 1.02 - 12.7 mm
Sheet and plate
 >= 400 MPa
@Thickness 12.7 - 50.8 mm
Plate; T451
 >= 400 MPa
@Thickness 12.7 - 25.4 mm
Sheet and plate
Tensile Strength, Yield 37.0 ksiAA; Typical
 >= 200 MPa
@Thickness 50.83 - 76.2 mm
Plate; T451
 >= 215 MPa
@Thickness 0.508 - 0.610 mm
Coiled sheet
 >= 215 MPa
@Thickness 0.508 - 0.610 mm
Sheet and plate
 >= 220 MPa
@Thickness 0.635 - 0.991 mm
Coiled sheet
 >= 220 MPa
@Thickness 0.635 - 0.991 mm
Sheet and plate
 >= 235 MPa
@Thickness 1.02 - 6.32 mm
Coiled sheet
 >= 235 MPa
@Thickness 1.02 - 12.7 mm
Sheet and plate
 >= 235 MPa
@Thickness 12.7 - 25.4 mm
Sheet and plate
 >= 250 MPa
@Thickness 6.35 - 12.7 mm
Plate; T451
 >= 250 MPa
@Thickness 12.7 - 50.8 mm
Plate; T451
Elongation at Break 8.0 %
@Thickness 50.83 - 76.2 mm
Plate; T451
 12 - 14 %
@Thickness 12.7 - 50.8 mm
Plate; T451
 14 %
@Thickness 0.508 - 0.610 mm
Coiled sheet
 14 %
@Thickness 0.635 - 0.991 mm
Coiled sheet
 14 %
@Thickness 0.508 - 0.610 mm
Sheet and plate
 14 %
@Thickness 0.635 - 0.991 mm
Sheet and plate
 14 %
@Thickness 12.7 - 25.4 mm
Sheet and plate
 15 %
@Thickness 1.02 - 6.32 mm
Coiled sheet
 15 %
@Thickness 6.35 - 12.7 mm
Plate; T451
 15 %
@Thickness 1.02 - 12.7 mm
Sheet and plate
 22 %
@Thickness 1.59 mm
AA; Typical
Modulus of Elasticity 10500 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Shear Strength 37.0 ksiAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 935 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.4 - 95 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu 3.9 - 5.0 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.20 - 0.80 %
Manganese, Mn 0.40 - 1.2 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.50 - 1.2 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Alclad Aluminum 2014-T6, T651
Alclad Aluminum 2014-T3
Alclad Aluminum 2014-O
Aluminum 2014-T4; 2014-T451
Aluminum 2014-O

MA2014AT4 / 8843

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.