MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2618-T61 (Includes Creep/Rupture Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92618; Aluminium 2618-T61; AA2618-T61
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.76 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 115AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 144Converted from Brinell Hardness Value
Hardness, Rockwell A 45.5Converted from Brinell Hardness Value
Hardness, Rockwell B 72Converted from Brinell Hardness Value
Hardness, Vickers 130Converted from Brinell Hardness Value
Tensile Strength, Ultimate 64.0 ksiAA; Typical
 34.0 MPa
@Temperature 371 °C
 52.0 MPa
@Temperature 316 °C
 90.0 MPa
@Temperature 260 °C
 221 MPa
@Temperature 204 °C
 345 MPa
@Temperature 149 °C
 427 MPa
@Temperature 100 °C
 441 MPa
@Temperature -28.0 °C
 441 MPa
@Temperature 24.0 °C
 462 MPa
@Temperature -80.0 °C
 538 MPa
@Temperature -196 °C
 350 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 360 MPa
@Thickness <=50.8 mm
Hand forgings; Short transverse
 360 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 365 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 380 MPa
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 380 MPa
@Thickness <=50.8 mm
Hand forgings; Long transverse
 380 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 380 MPa
@Thickness <=63.5 mm
Rolled rings; Tangential
 380 MPa
@Thickness <=63.5 mm
Rolled rings; Axial
 385 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 395 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 400 MPa
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 400 MPa
@Thickness <=50.8 mm
Hand forgings; Longitudinal
Tensile Strength, Yield 54.0 ksiAA; Typical
 270 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 275 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 285 MPa
@Thickness <=63.5 mm
Rolled rings; Tangential
 285 MPa
@Thickness <=63.5 mm
Rolled rings; Axial
 290 MPa
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 290 MPa
@Thickness <=50.8 mm
Hand forgings; Long transverse
 290 MPa
@Thickness <=50.8 mm
Hand forgings; Short transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 310 MPa
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 310 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 315 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 325 MPa
@Thickness <=50.8 mm
Hand forgings; Longitudinal
 24.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 31.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 62.0 MPa
@Strain 0.2 %,
Temperature 260 °C
 179 MPa
@Strain 0.2 %,
Temperature 204 °C
 303 MPa
@Strain 0.2 %,
Temperature 149 °C
 372 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 372 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 372 MPa
@Strain 0.2 %,
Temperature 100 °C
 379 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 10 %
@Temperature -28.0 °C
 10 %
@Temperature 24.0 °C
 10 %
@Temperature 100 °C
 11 %
@Temperature -80.0 °C
 12 %
@Temperature -196 °C
 14 %
@Temperature 149 °C
 24 %
@Temperature 204 °C
 50 %
@Temperature 260 °C
 80 %
@Temperature 316 °C
 120 %
@Temperature 371 °C
 4.0 %
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 4.0 %
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 4.0 %
@Thickness <=50.8 mm
Hand forgings; Short transverse
 4.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 4.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 5.0 %
@Thickness <=50.8 mm
Hand forgings; Long transverse
 5.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 5.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 5.0 %
@Thickness <=63.5 mm
Rolled rings; Axial
 6.0 %
@Thickness <=63.5 mm
Rolled rings; Tangential
 7.0 %
@Thickness <=50.8 mm
Hand forgings; Longitudinal
 7.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 7.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 10 %
@Diameter 12.7 mm
AA; Typical
Creep Strength 14.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.5% creep
 15.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.1% creep
 17.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
1% creep
 19.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.2% creep
 26.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.5% creep
 26.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.1% creep
 28.0 MPa
@Temperature 315 °C,
Time 360000 sec
1% creep
 38.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.2% creep
 41.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.5% creep
 41.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.1% creep
 45.0 MPa
@Temperature 315 °C,
Time 36000 sec
1% creep
 45.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.2% creep
 48.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.2% creep
 48.0 MPa
@Temperature 315 °C,
Time 360 sec
0.1% creep
 52.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.1% creep
 55.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.5% creep
 55.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.5% creep
 55.0 MPa
@Temperature 315 °C,
Time 360 sec
0.2% creep
 62.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
1% creep
 62.0 MPa
@Temperature 315 °C,
Time 3600 sec
1% creep
 69.0 MPa
@Temperature 315 °C,
Time 360 sec
0.5% creep
 69.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.2% creep
 83.0 MPa
@Temperature 315 °C,
Time 360 sec
1% creep
 83.0 MPa
@Temperature 260 °C,
Time 36000 sec
0.1% creep
 90.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.5% creep
 90.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.1% creep
 97.0 MPa
@Temperature 260 °C,
Time 360000 sec
1% creep
 110 MPa
@Temperature 260 °C,
Time 36000 sec
0.2% creep
 115 MPa
@Temperature 260 °C,
Time 3600 sec
0.1% creep
 125 MPa
@Temperature 260 °C,
Time 36000 sec
0.5% creep
 130 MPa
@Temperature 260 °C,
Time 36000 sec
1% creep
 130 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.2% creep
 140 MPa
@Temperature 260 °C,
Time 3600 sec
0.2% creep
 140 MPa
@Temperature 205 °C,
Time 360000 sec
0.1% creep
 145 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.5% creep
 145 MPa
@Temperature 260 °C,
Time 3600 sec
0.5% creep
 145 MPa
@Temperature 260 °C,
Time 360 sec
0.1% creep
 150 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
1% creep
 150 MPa
@Temperature 260 °C,
Time 3600 sec
1% creep
 150 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
0.1% creep
 160 MPa
@Temperature 260 °C,
Time 360 sec
0.2% creep
 165 MPa
@Temperature 260 °C,
Time 360 sec
0.5% creep
 165 MPa
@Temperature 205 °C,
Time 360000 sec
0.2% creep
 170 MPa
@Temperature 260 °C,
Time 360 sec
1% creep
 170 MPa
@Temperature 205 °C,
Time 36000 sec
0.1% creep
 180 MPa
@Temperature 205 °C,
Time 360000 sec
0.5% creep
 185 MPa
@Temperature 205 °C,
Time 360000 sec
1% creep
 185 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
0.2% creep
 185 MPa
@Temperature 177 °C,
Time 360000 sec
0.1% creep
 195 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
0.5% creep
 200 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
1% creep
 200 MPa
@Temperature 205 °C,
Time 36000 sec
0.2% creep
 205 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.1% creep
 205 MPa
@Temperature 205 °C,
Time 3600 sec
0.1% creep
 215 MPa
@Temperature 205 °C,
Time 36000 sec
0.5% creep
 220 MPa
@Temperature 205 °C,
Time 36000 sec
1% creep
 220 MPa
@Temperature 177 °C,
Time 360000 sec
0.2% creep
 220 MPa
@Temperature 177 °C,
Time 36000 sec
0.1% creep
 235 MPa
@Temperature 177 °C,
Time 360000 sec
0.5% creep
 235 MPa
@Temperature 205 °C,
Time 3600 sec
0.2% creep
 240 MPa
@Temperature 177 °C,
Time 360000 sec
1% creep
 240 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.2% creep
 240 MPa
@Temperature 150 °C,
Time 360000 sec
0.1% creep
 240 MPa
@Temperature 205 °C,
Time 360 sec
0.1% creep
 250 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.5% creep
 250 MPa
@Temperature 205 °C,
Time 3600 sec
0.5% creep
 250 MPa
@Temperature 177 °C,
Time 36000 sec
0.2% creep
 255 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
1% creep
 255 MPa
@Temperature 205 °C,
Time 3600 sec
1% creep
 255 MPa
@Temperature 205 °C,
Time 360 sec
0.2% creep
 255 MPa
@Temperature 177 °C,
Time 3600 sec
0.1% creep
 260 MPa
@Temperature 177 °C,
Time 36000 sec
0.5% creep
 270 MPa
@Temperature 205 °C,
Time 360 sec
0.5% creep
 270 MPa
@Temperature 150 °C,
Time 360000 sec
0.2% creep
 270 MPa
@Temperature 150 °C,
Time 36000 sec
0.1% creep
 275 MPa
@Temperature 177 °C,
Time 36000 sec
1% creep
 275 MPa
@Temperature 177 °C,
Time 3600 sec
0.2% creep
 285 MPa
@Temperature 205 °C,
Time 360 sec
1% creep
 285 MPa
@Temperature 177 °C,
Time 360 sec
0.1% creep
 290 MPa
@Temperature 150 °C,
Time 360000 sec
0.5% creep
 290 MPa
@Temperature 150 °C,
Time 3600 sec
0.1% creep
 295 MPa
@Temperature 177 °C,
Time 3600 sec
0.5% creep
 295 MPa
@Temperature 150 °C,
Time 36000 sec
0.2% creep
 295 MPa
@Temperature 177 °C,
Time 360 sec
0.2% creep
 305 MPa
@Temperature 150 °C,
Time 360000 sec
1% creep
 305 MPa
@Temperature 177 °C,
Time 3600 sec
1% creep
 315 MPa
@Temperature 150 °C,
Time 36000 sec
0.5% creep
 315 MPa
@Temperature 177 °C,
Time 360 sec
0.5% creep
 315 MPa
@Temperature 150 °C,
Time 3600 sec
0.2% creep
 315 MPa
@Temperature 150 °C,
Time 360 sec
0.1% creep
 325 MPa
@Temperature 150 °C,
Time 36000 sec
1% creep
 325 MPa
@Temperature 177 °C,
Time 360 sec
1% creep
 330 MPa
@Temperature 150 °C,
Time 3600 sec
0.5% creep
 330 MPa
@Temperature 150 °C,
Time 360 sec
0.2% creep
 340 MPa
@Temperature 150 °C,
Time 3600 sec
1% creep
 345 MPa
@Temperature 150 °C,
Time 360 sec
1% creep
 345 MPa
@Temperature 150 °C,
Time 360 sec
0.5% creep
Rupture Strength 20.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
 32.0 MPa
@Temperature 315 °C,
Time 360000 sec
 52.0 MPa
@Temperature 315 °C,
Time 36000 sec
 62.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
 69.0 MPa
@Temperature 315 °C,
Time 3600 sec
 97.0 MPa
@Temperature 315 °C,
Time 360 sec
 105 MPa
@Temperature 260 °C,
Time 360000 sec
 140 MPa
@Temperature 260 °C,
Time 36000 sec
 160 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
 165 MPa
@Temperature 260 °C,
Time 3600 sec
 185 MPa
@Temperature 260 °C,
Time 360 sec
 195 MPa
@Temperature 205 °C,
Time 360000 sec
 205 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
 230 MPa
@Temperature 205 °C,
Time 36000 sec
 250 MPa
@Temperature 177 °C,
Time 360000 sec
 255 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
 260 MPa
@Temperature 205 °C,
Time 3600 sec
 285 MPa
@Temperature 177 °C,
Time 36000 sec
 290 MPa
@Temperature 205 °C,
Time 360 sec
 305 MPa
@Temperature 150 °C,
Time 360000 sec
 310 MPa
@Temperature 177 °C,
Time 3600 sec
 340 MPa
@Temperature 150 °C,
Time 36000 sec
 340 MPa
@Temperature 177 °C,
Time 360 sec
 360 MPa
@Temperature 150 °C,
Time 3600 sec
 380 MPa
@Temperature 150 °C,
Time 360 sec
Modulus of Elasticity 10800 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Compressive Strength 370 MPa
Poissons Ratio 0.33
Fatigue Strength 18000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaCalculated
Shear Strength 38.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000470 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.6 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.2 µm/m-°C
@Temperature 20.0 - 200 °C
 24.0 µm/m-°C
@Temperature 20.0 - 300 °C
average
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.875 J/g-°C
Thermal Conductivity 146 W/m-K
Melting Point 1020 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 1020 °FAA; Typical
Liquidus 1180 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Solution Temperature 985 °F
Aging Temperature 390 °Ffor 20 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 92.4 - 94.9 %As remainder
Copper, Cu 1.9 - 2.7 %
Iron, Fe 0.90 - 1.3 %
Magnesium, Mg 1.3 - 1.8 %
Nickel, Ni 0.90 - 1.2 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.10 - 0.25 %
Titanium, Ti 0.04 - 0.10 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 7178-T6; 7178-T651 (Included Creep/Rupture Data)
Aluminum 2219-T87 (Extended Creep-Rupture Data)
Aluminum 2618-T61
Aluminum 2618-T6
AISI 8620H Steel, quenched from 900°C (1650°F), tempered at 650°C (1200°F), Low temp impact properties

MA2618T61a / 170635

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.