MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Arlon Electronic Materials 91ML Low-Cost Halogen-Free Thermally Conductive Epoxy
Categories: Polymer; Thermoset; Epoxy; Epoxy, Thermally Conductive

Material Notes: Thermally conductive, multilayerable laminate and prepreg circuit board material. Available in various resin content percentages.

Arlon 91ML ceramic filled thermally conductive multifunctional epoxy laminate and prepreg products provide a low-cost, lead-free solder compatible system with enhanced heat transfer characteristics for multilayer PWBs for applications requiring thermal management throughout the entire board volume.

  • Engineered for use with metal backing for producing Metal-Clad PCBs
  • RoHS/WEEE compliant

Typical Applications:

  • High brightness LEDs
  • DC-DC power converters
  • Automotive electronics
  • Electronic designs with limited thermal management alternatives

Information provided by ARLON Electronic Materials.

Vendors: Arlon Materials for Electronics (MED) is a major manufacturer of specialty high performance laminate and prepreg materials for use in a wide variety of printed circuit board (PCB) applications and in several distinctive markets.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.05 g/ccASTM D792 Method A
Water Absorption 0.13 %IPC TM-650 2.6.2.1
 
Mechanical PropertiesOriginal ValueComments
Flexural Strength 31.0 - 49.0 ksiIPC TM-650 2.4.4
Peel Strength 4.50 pliTo Copper (1 oz/35 micron); After Process Solutions; IPC TM-650 2.4.8
 5.00 pliTo Copper (1 oz/35 micron); After Thermal Stress; IPC TM-650 2.4.8
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.20e+13 ohm-cmE24/125; IPC TM-650 2.5.17.1
 2.80e+14 ohm-cmC96/35/90; IPC TM-650 2.5.17.1
Surface Resistance 1.70e+13 ohmE24/125; IPC TM-650 2.5.17.1
 4.40e+13 ohmC96/35/90; IPC TM-650 2.5.17.1
Dielectric Constant 5.5
@Frequency 1e+6 Hz
IPC TM-650 2.5.5.3
Dielectric Strength >= 1000 V/milIPC TM-650 2.5.6.2
Dielectric Breakdown 43000 VIPC TM-650 2.5.6
Dissipation Factor 0.017
@Frequency 1e+6 Hz
IPC TM-650 2.5.5.3
Arc Resistance 193 secIPC TM-650 2.5.1
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.0 µm/m-°Cx,y direction; IPC TM-650 2.4.41
CTE, linear, Transverse to Flow 36.0 µm/m-°C
@Temperature <=160 °C
z (< Tg); IPC TM-650 2.4.24
 192 µm/m-°C
@Temperature >=160 °C
z (> Tg); IPC TM-650 2.4.24
Thermal Conductivity 1.00 W/m-KZ-axis; ASTM E1461
 1.90 W/m-KX/Y-axis; ASTM E1461
Glass Transition Temp, Tg 160 °CTMA; IPC TM-650 2.4.24
 170 °CDSC; IPC TM-650 2.4.25
Decomposition Temperature 354 °COnset; IPC TM-650 2.3.41
 368 °C5 percent; IPC TM-650 2.3.41
Flammability, UL94 V-0
 
Descriptive Properties
Dielectric Withstand Voltage (VDC)> 5000HiPot; IPC TM-650 2.5.7.2
IPC Delamination - T260 (minutes)> 60IPC TM-650 2.4.24.1
IPC Delamination - T288 (minutes)> 30IPC TM-650 2.4.24.1
IPC Delamination - T300 (minutes)> 10IPC TM-650 2.4.24.1
Z-Axis Expansion (%)2.6IPC TM-650 2.4.24 (50-260°C)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Arlon Electronic Materials 99ML Thermally Conductive Epoxy
Aremco Aremco-Bond™ 525 Electrically & Thermally Conductive Material, Silver Filled
Parker Chomerics THERM-A-GAP™ 976 Thermally Conductive Gap Filler Pad
Park Aerospace Nelco® NH9338 PTFE Laminate, Woven-Glass and Ceramic Reinforced
Atom Adhesives AA-SUPERTHERM 195 Epoxy Adhesive

PARLM9859 / 149012

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.