MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Silver, Ag
Categories: Metal; Nonferrous Metal; Precious Metal; Silver Alloy; Pure Element

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 10.491 g/cc
 9.00 g/cc
@Temperature 1300 °C
Liquid
 9.10 g/cc
@Temperature 1195 °C
Liquid
 9.20 g/cc
@Temperature 1092 °C
Liquid
 9.26 g/cc
@Temperature 1000 °C
Liquid
 9.30 g/cc
@Temperature 960.5 °C
Liquid
Vapor Pressure 1.013 bar
@Temperature 1304 °C
 10.13 bar
@Temperature 1510 °C
 101.3 bar
@Temperature 1783 °C
 1013 bar
@Temperature 2163 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 107.86821995
Atomic Number 47
Thermal Neutron Cross Section 63 barns/atom
X-ray Absorption Edge 0.4858 ÅK
 3.23824 ÅLI
 3.49478 ÅLII
 3.67288 ÅLIII
Electrode Potential 0.799 V
Electronegativity 1.93Pauling
Ionic Radius 0.89 ÅCrystal Ionic Radius for Valence +2
 1.26 ÅCrystal Ionic Radius for Valence +1
Electrochemical Equivalent 4.025 g/A/h
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 25Annealed
Tensile Strength, Ultimate 140 MPaAnnealed
Modulus of Elasticity 76.0 GPa
Poissons Ratio 0.37Annealed
 0.39Hard drawn
Shear Modulus 27.8 GPaCalculated; Annealed
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000155 ohm-cm
Magnetic Susceptibility 2.0e-7cgs/g
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 105 J/g
Heat of Vaporization 2332 J/g
CTE, linear 19.6 µm/m-°C
@Temperature 20.0 - 100 °C
 19.9 µm/m-°C
@Temperature 0.000 - 250 °C
 20.6 µm/m-°C
@Temperature 0.000 - 500 °C
 22.4 µm/m-°C
@Temperature 0.000 - 900 °C
Specific Heat Capacity 0.234 J/g-°C
Thermal Conductivity 419 W/m-K
Melting Point 961.93 °C
Boiling Point 2162 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.055
@Temperature 700 °C
Reflection Coefficient, Visible (0-1) 0.90
 
Component Elements PropertiesOriginal ValueComments
Silver, Ag 100 %
 
Descriptive Properties
CAS Number7440-22-4

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum, Al
Gold, Au
Copper, Cu; Annealed
Americium, Am
Iron, Fe

AMEAg00 / 2

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.