MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC LNP™ THERMOCOMP™ Compound MX89510 Polypropylene, Unspecified (PP, Unspecified)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: LNP THERMOCOMP MX89510 compound is based on Polypropylene (PP) resin containing 10% glass fiber, 10% glass bead.

Features: High Stiffness,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.02 g/ccASTM D792
Density 1.01 g/ccASTM D792
Moisture Absorption 0.0200 %23°C/50% RH/24 hrs; ASTM D570
 0.0200 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0080 - 0.020 cm/cm24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0090 - 0.030 cm/cm24hrs; ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 48.0 MPa5 mm/min; ISO 527
 52.0 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 50.0 MPa5 mm/min; ISO 527
 52.0 MPa5 mm/min; ASTM D638
Elongation at Break 3.4 %5 mm/min; ASTM D638
 3.4 %5 mm/min; ISO 527
Elongation at Yield 2.9 %5 mm/min; ISO 527
 3.0 %5 mm/min; ASTM D638
Tensile Modulus 3540 MPa1 mm/min; ISO 527
 3820 MPa50 mm/min; ASTM D638
Flexural Strength 76.0 MPaISO 178
 80.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2800 MPa1.3 mm/min, 50 mm span; ASTM D790
 2950 MPa2 mm/min; ISO 178
Izod Impact Notched 21.0 JASTM D256
Izod Impact, Unnotched 368 J/mASTM D4812
Izod Impact, Notched (ISO) 2.00 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 22.0 kJ/m²80*10*4; ISO 180/1U
Dart Drop, Total Energy 4.00 JASTM D3763
Impact Test 1.00 JMultiaxial Impact; ISO 6603
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 43.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM D696
CTE, linear, Transverse to Flow 120 µm/m-°C
@Temperature -30.0 - 30.0 °C
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 153 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 156 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 119 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 131 °C
@Thickness 3.20 mm
unannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Zone 2 215 - 225 °C
Zone 3 240 - 250 °C
Melt Temperature 225 - 250 °CInjection Molding
Mold Temperature 30.0 - 50.0 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH81735 / 289682

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.