MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
NOVA Chemicals Novapol® TF-0219-E Hexene LLDPE Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Hexene, Film Grade

Material Notes: Exceptional toughens, Low gel level

Applications: Cast stretch wrap

Additives: High temperature A/O

Film properties are typical of cast film extruded at a melt temperature of 540°F, and a line speed of 1220 ft/min.

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.918 g/ccASTM D792
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 8.00 MPaASTM D882
Film Tensile Strength at Yield, TD 8.00 MPaASTM D882
Film Elongation at Break, MD 550 %ASTM D882
Film Elongation at Break, TD 840 %ASTM D882
Secant Modulus, MD 0.140 GPaat 1%; ASTM D882
Secant Modulus, TD 0.150 GPaat 1%; ASTM D882
Impact 185J/mm; NOVA Chemicals Puncture test
Elmendorf Tear Strength, MD 16.0 g/micronASTM D1922
Elmendorf Tear Strength, TD 30.0 g/micronASTM D1922
Dart Drop 8.00 g/micronF50, ASTM D1709/A
Film Tensile Strength at Break, MD 45.0 MPaASTM D882
Film Tensile Strength at Break, TD 30.0 MPaASTM D882
 
Optical PropertiesOriginal ValueComments
Haze 2.0 %ASTM D1003
Gloss 90 %at 45°; 1 mil; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for AISI 1000 Series Steel
Latrobe LSS™ 4140 Alloy Steel (AISI 4140)
HY-80 Steel
HY-100 Steel
AISI 4140 Steel, normalized at 870°C (1600°F), reheated to 845°C (1550°F), oil quenched, 705°C (1300°F) temper, 25 mm (1 in.) round

PNOVA148 / 55049

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.