MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
BASF 3D Ultrafuse® PAHT CF15 Fused Fillament, Dry
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Components: High temperature Polyamide based filament filled with 15% carbon fibers for Fused Filament Fabrication.

Product Description: PAHT CF15 is a high-performance 3D printing filament that opens new application fields in FFF printing. In parallel to its advanced mechanical properties, dimensional stability, and chemical resistance, it has very good processability. It works in any FFF printer with a hardened nozzle. In addition to that, it is compatible with water-soluble support material and HiPS, which allow printing complex geometries that work in challenging environments. PAHT CF15 has high heat resistance up to 130 °C and low moisture absorption.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.232 g/ccPrinted Part; ISO 1183-1
Melt Flow 51.9904 g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1133
Storage Temperature 15.0 - 25.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 18.2 MPaZX: Upright; ISO 527
 103.2 MPaXY: Flat; ISO 527
Elongation at Break 0.50 %ZX: Upright; ISO 527
 1.8 %XY: Flat; ISO 527
Modulus of Elasticity 3.532 GPaYoung's, ZX: Upright; ISO 527
 8.386 GPaYoung's, XY: Flat; ISO 527
Flexural Strength 50.8 MPaZX: Upright; ISO 178
 160.7 MPaXY: Flat; ISO 178
 171.8 MPaXZ: On its edge; ISO 178
Flexural Modulus 2715 MPaZX: Upright; ISO 178
 7669 MPaXZ: On its edge; ISO 178
 8258 MPaXY: Flat; ISO 178
Flexural Strain at Break 1.8 %ZX: Upright; ISO 178
 2.4 %XY: Flat; ISO 178
 2.8 %XZ: On its edge; ISO 178
Izod Impact, Notched (ISO) 4.90 kJ/m²XY: Flat; ISO 180
 5.10 kJ/m²XZ: On its edge; ISO 180
Izod Impact, Unnotched (ISO) 2.90 kJ/m²ZX: Upright; ISO 180
 16.4 kJ/m²XY: Flat; ISO 180
 18.1 kJ/m²XZ: On its edge; ISO 180
Charpy Impact Unnotched 2.90 kJ/m²ZX: Upright; ISO 179-2
 19.3 kJ/m²XZ: On its edge; ISO 179-2
 20.6 kJ/m²XY: Flat; ISO 179-2
Charpy Impact, Notched 1.30 kJ/m²ZX: Upright; ISO 179-2
 3.90 kJ/m²XZ: On its edge; ISO 179-2
 4.80 kJ/m²XY: Flat; ISO 179-2
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 160000 ohm-cmZX: Upright; IEC 62631-3-1
 3.20e+7 ohm-cmXY: Flat; IEC 62631-3-1
Surface Resistance 970000 ohmXY: Flat; IEC 62631-3-2
 1.80e+6 ohmZX: Upright; IEC 62631-3-2
 
Thermal PropertiesOriginal ValueComments
Melting Point 234 °CISO 11357-3
Crystallization Temperature 180 °CISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 145 °CISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °CISO 75-2
Glass Transition Temp, Tg 70.0 °CISO 11357-2
 
Processing PropertiesOriginal ValueComments
Processing Temperature 100 - 120 °CBed, Bed Material: PEI or Glass
Nozzle Temperature 260 - 280 °C
Drying Temperature 70.0 °Cin a hot air dryer, ensure printability
 80.0 °Cin a hot air dryer, best mechanical part properties
Dry Time 4.00 - 16.0 hour
 40.0 hour
Shelf Life 12.0 Month
 
Descriptive Properties
Nozzle Diameter=0.6 mmRuby or Hardened
Print speed30-80 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASF3D012 / 312253

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.