MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Morgan Advanced Ceramics Alumina AL998A Aluminum Oxide Ceramic
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: High purity alumina with a minimum purity of 99.8%. Specifically developed for semiconductor processing applications.

Prime Features:

  • High resistance to semiconductor etch chemistries
  • Excellent chemical resistance to acids, bases and organics
  • Small grain size, low porosity, high polishability. High volume resistivity
  • Superior mechanical wear resistance
  • Less than 100 ppm soda and silica impurity levels
  • Maintains surface integrity in corrosive environments
Typical applications:
  • Semiconductor components for etch, PVD, CVD, CMP, implant and litho processes
  • High power laser insulators
  • Wear-resistant rotary components
  • Blood seals and valves
  • Piston & sleeve pump sets
  • High vacuum components
Production Capabilities:
  • Process application suppori
  • Isostatic, monostatic & uniaxial pressing
  • Lapping & polishing to 2 microinch Ra
  • Manual, CNC and high precision machining
  • Straight right cylinder straightness to <10 microinch per inch and roundness to <20 microinches

Information provided by Morgan Advanced Materials

Key Words: AL998A
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 3.94 g/ccASTM C373
Water Absorption >= 0.0040 %ASTM C373
Grain Size >= 6.0 µmASTM E112-96
Permeability >= 1.0e-10Torr-L/sec; He Leak detection
Weibull Modulus 25ASTM C1161, C1239
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell HR45N 86
Modulus of Elasticity 391 GPaASTM C848
Flexural Strength 361 MPa
@Temperature 20.0 °C
3-point bend
Poissons Ratio 0.19ASTM C848
Fracture Toughness 4.30 - 4.60 MPa-m½NIST Indentation
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.00e+7 ohm-cm
@Temperature 700 °C
ASTM D257
 4.00e+11 ohm-cm
@Temperature 300 °C
ASTM D257
 1.00e+14 ohm-cm
@Temperature 20.0 °C
ASTM D257
Dielectric Constant 9.6
@Frequency 1e+6 Hz
ASTM D2520
Dielectric Strength >= 23.0 kV/mmASTM D149
Dissipation Factor 0.00030
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 7.40 µm/m-°C
@Temperature 40.0 - 400 °C
ASTM C372
 8.10 µm/m-°C
@Temperature 40.0 - 800 °C
ASTM C372
Specific Heat Capacity 0.911 J/g-°C
@Temperature 100 °C
ASTM E1461
Thermal Conductivity 27.0 W/m-K
@Temperature 100 °C
ASTM C408
 
Component Elements PropertiesOriginal ValueComments
Al2O3 >= 99.8 %
 
Descriptive Properties
Colorivory
Content<100 ppmImpurities (as SiO2)
Inclusions0, 3x visual, .0.8mm dia
Thermal Shock ResistanceΔT = 212°CASTM C1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

CMORF5018 / 200256

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.