MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

(Viewing data as-entered. Click here to return)
Chemical Concepts Chem-Set™ TrimGrip Acrylic Adhesive
Categories: Polymer; Adhesive; Thermoset; Acrylic/Cyanoacrylate Adhesive

Material Notes: Chem-Set TrimGrip (formerly known as TrimBonder parts 74401, 74301, and 74201) is an adhesive bonding system that permanently bonds trimboards, metals, synthetic wood, and PVC. Fetures include ease of sanding and curing in just 30 minutes.

Uses:

  • Fill Gaps - Use TrimGrip™ adhesive to fill the gaps left between edge of house and trim board.
  • Fill Nail Holes - Fill nail holes simply and quickly with TrimGrip™ adhesive, available in a convenient 250ml cartridge. Fill the hole with adhesive, wipe away any excess for a clean, smooth surface.
  • Window/Door Trim Bond trim board around windows or doors for a custom look.
  • Fascia Trim Boards Bond and fill all CPVC trim boards (such as AZEK®, Koma®, Fypon®, etc).
  • Fill Joints - Fill in joints that are created when trim boards meet.
  • Millwork Uses: Laminating -TrimGrip™ adhesive can be used in a simple process in taking 4 x 18 sheets of CPVC board and laminate to create larger dimensional thicknesses, allowing millwork shops to then cut multiple parts quickly, easily and economically.
  • Pergolas - Pergolas are great to add to any house to help diffuse light.
  • Columns - Bond column wraps together using TrimGrip™ adhesive for the "no nail hole look" or laminate pieces of CPVC together to millwork a custom column.
  • Cupolas - Cupolas are a great addition to any house, an added feature that can be customized to any design idea. These made of CPVC are low maintenance, perfect for venting or non-venting options.
  • Railings - Custom deck railing systems can be achieved, even curved railings when using TrimGrip™ adhesive.
  • Trellis - Decorative lattice work can be assembled with a "no nail hole look" by using TrimGrip™ adhesive to create a nail free smooth lattice for the trellis.
  • Bead Board - For a finished porch, use TrimGrip™ adhesive to bond CPVC bead board along the ceiling. Add the finishing touches to the ceiling list by creating a medallion. Works both outdoors in the porch entrance and inside in the living room.
  • Doors - Bonding gate doors for the entrance or opening to a garden by using TrimGrip™ adhesive to fill gaps and laminating boards together. Also, millwork custom garage doors.
  • Outdoor Furniture - Bonding gate doors for the entrance or opening to a garden by using TrimGrip™ adhesive to fill gaps and laminating boards together. Also, millwork custom garage doors.
  • Pediments & Others - Custom designed window dressings. Laminate boards together for thicker dimensions using TrimGrip™ Adhesive.
  • Mailboxes - Use TrimGrip™ Adhesive to customize mailboxes with a planter box or newspaper slot.

Information provided by Chemical Concepts™.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.80 lb/galuncured, mixed
Solids Content 100 %Cured 7 days @75°F
Viscosity 18000 cPadhesive, uncured
 30000 cPuncured, mixed
 45000 cPactivator, uncured
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 75
Elongation at Break 5.0 - 15 %cured 7 days @ 75°F
Adhesive Bond Strength 586 psivs. CPVC; substrate failure, cured 7 days @ 75°F; ASTM D1002
 1300 psivs. PVC; substrate failure, cured 7 days @ 75°F; ASTM D1002
 2354 psiAl/Al; cured 7 days @ 75°F; ASTM D1002
Peel Strength 15.0 - 20.0 pliCured 7 days @75°F; ASTM D 1876
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 160 °F
Minimum Service Temperature, Air -40.0 °F
Flash Point 51.0 °F
 
Processing PropertiesOriginal ValueComments
Cure Time 2.00 hourFunctional. At room temp
 24.0 hourFull
Working Life 5.00 - 8.00 min
@Temperature 22.2 °C
 
Descriptive Properties
Colorwhite, uncured
Gap Filling0.375 inches, cured 7 days @ 75°F
Impact Resistance20 ft. lb/in, cured 7 days @ 75°F, STM D950
Mix Ratio1:1, uncured
Tack Free Time18-20 min @ 72°F
WeightAdhesive:9.5 lbs/gal. Activator: 8.1 lbs/gal. Uncured

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1059 Steel

PCHEMI975 / 232160

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.