MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Ovako 29MnCrB5-2* SB28M13CB/9667 Steel, Quench & Tempering
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: General Information: WR-Steel(Wear resistant ) WR-steel, stands for wear-resistant steel. This group of steel includes a broad range of grades with a wide range of hardness levels 350 – 650 HV, dimensions and steel grades designed to give you a wear-resistant advantage when making product exposed to a high degree of wear and where service life is important. WR-steels are characterized by consistent properties and cost effectiveness due to optimized alloy content for different end applications. Boron grade 29MnCrB5-2 is a non-standardized grade located in between 27MnCrB5-2 and 33MnCrB5-2. It is suitable for wear parts, but may be heat-treated for good toughness if needed. A tight chemical composition ensures repeatable heat-treatment response.

Information provided by Ovako

Key Words: 27MnCrB5-2, 33MnCrB5-2, 15B35H, SB9667
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 950 - 1025 MPa
@Thickness 14.0 mm
All formats
Tensile Strength, Yield >= 880 MPa
@Thickness 14.0 mm
All formats
Elongation at Break 12 %
@Thickness 14.0 mm
All formats
Reduction of Area 45 %
@Thickness 14.0 mm
All formats
Modulus of Elasticity 210 GPa
Poissons Ratio 0.30
Shear Modulus 80.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
Thermal Conductivity 40.0 - 45.0 W/m-KAmbient temperature
Transformation Temperature 368 °CMS
 720 °CAC1
 781 °CAC3
 
Component Elements PropertiesOriginal ValueComments
Boron, B 0.0020 - 0.0050 %
Carbon, C 0.28 - 0.33 %
Chromium, Cr 0.25 - 0.60 %
Iron, Fe 97.11 - 98.22 %As Balance
Manganese, Mn 1.1 - 1.5 %
Phosphorus, P <= 0.030 %
Silicon, Si 0.15 - 0.40 %
Sulfur, S <= 0.030 %
 
Descriptive Properties
WeldabilityCEV 0.62max
 Pcm 0.41max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 15B37H Carbon Steel, Composition Spec
AISI 15B35H Carbon Steel, Composition Spec
AISI 15B21H Carbon Steel, Composition Spec
Ovako 27MnCrB5-2 SB29M13CB (SB9667) Steel
Ovako 27MnCrB5-2 SB28M12CB (SB9652) Steel, +AR

NOVAKO220 / 234519

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.