MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
AISI Type 420F(Se) Stainless Steel, annealed bar
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes:

Key Words: UNS S42023, AMS 5620, SAE J405 (51420FSe), martensitic
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 220
Hardness, Rockwell C 18Converted from Brinell Hardness. Value below normal Rockwell C Hardness range, for comparison only.
Tensile Strength, Ultimate 655 MPa
Tensile Strength, Yield 380 MPa
@Strain 0.2 %
Elongation at Break 22 %in 50 mm
Modulus of Elasticity 200 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000550 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.3 µm/m-°C
@Temperature 0.000 - 100 °C
 12.2 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 25.1 W/m-K
@Temperature 27.0 °C
Melting Point 1455 - 1510 °C
Solidus 1455 °C
Liquidus 1510 °C
Maximum Service Temperature, Air 620 °CContinuous Service
 735 °CIntermittent
 
Component Elements PropertiesOriginal ValueComments
Carbon, C >= 0.15 %
Chromium, Cr 13 %
Iron, Fe 84 %
Manganese, Mn <= 1.0 %
Molybdenum, Mo <= 0.60 %Optional
Phosphorus, P <= 0.040 %
Selenium, Se >= 0.15 %
Silicon, Si <= 1.0 %
Sulfur, S >= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type 420F Stainless Steel, annealed bar
420 Stainless Steel
420 Stainless Steel, hardened and tempered bar
AISI Type 420F Stainless Steel, annealed and cold drawn bar
420 Stainless Steel, soft bright tempered

MQ420T / 13081

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.