MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Melos Mecoline IS RDX 1201 F Irradiation cross-linkable, halogen-free, flame retardant compound
Categories: Polymer; Thermoplastic

Material Notes: Irradiation cross-linkable, halogen-free, flame retardant compound

Compound class: Insulation/Sheathing

Compound category: RDX

Flame retardant: MDH

Standards: DIN/VDE DKE AK 411.2.3; TÜV 2PfG 1169/08.2007

Typical applications: A flame retardant, halogen-free and low smoke, oil resistant compound. Max. operating temperature 125°C

Features: Flame retardant; Halogen-free; Low smoke; Oil resistant; High temperature resistant

Information provided by Melos

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.38 g/ccpressed plaques; DIN EN ISO 1183-1A
Melt Flow 8.0 g/10 min
@Load 21.6 kg,
Temperature 165 °C
DIN EN ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 45pressed plaques; DIN ISO 7619-1
Tensile Strength 11.5 MPaextruded tapes; IEC 60811-501
 18.0 MPacross-linked plaques or tapes, 80kGy; IEC 60811-501
 9.304 MPa
@Temperature 100 °C,
Time 86400 sec
extruded tapes, Fluid IRM 902; IEC 60811-404
 9.77 MPa
@Temperature 23.0 °C,
Time 605000 sec
extruded tapes, 1N Oxalic acid; IEC 60811-404
 10.478 MPa
@Temperature 23.0 °C,
Time 605000 sec
extruded tapes, 1N NaOH; IEC 60811-404
 12.18 MPa
@Temperature 180 °C,
Time 518000 sec
extruded tapes, After ageing in air oven; IEC 60811-401
 12.78 MPa
@Temperature 165 °C,
Time 1.73e+6 sec
extruded tapes, After ageing in air oven; IEC 60811-401
 13.8 MPa
@Temperature 155 °C,
Time 3.629e+6 sec
extruded tapes, After ageing in air oven; IEC 60811-401
Elongation at Break 213 %cross-linked plaques or tapes, 80kGy; IEC 60811-501
 229 %extruded tapes; IEC 60811-501
 10 %
@Temperature 200 °C,
Time 900 sec
Hot set test, after unloading, 0.2 Mpa; IEC 60811-507
 15 %
@Temperature 250 °C,
Time 900 sec
Hot set test, after unloading, 0.2 Mpa; IEC 60811-507
 25 %
@Temperature 200 °C,
Time 900 sec
Hot set test, under load, 0.2 MPa; IEC 60811-507
 50 %
@Temperature 250 °C,
Time 900 sec
Hot set test, under load, 0.2 MPa; IEC 60811-507
 164.88 %
@Temperature 100 °C,
Time 86400 sec
extruded tapes, Fluid IRM 902; IEC 60811-404
 171.98 %
@Temperature 165 °C,
Time 1.73e+6 sec
extruded tapes, After ageing in air oven; IEC 60811-401
 180.7 %
@Temperature 155 °C,
Time 3.629e+6 sec
extruded tapes, After ageing in air oven; IEC 60811-401
 182.74 %
@Temperature 180 °C,
Time 518000 sec
extruded tapes, After ageing in air oven; IEC 60811-401
 254.88 %
@Temperature 23.0 °C,
Time 605000 sec
extruded tapes, 1N NaOH; IEC 60811-404
 255.8 %
@Temperature 23.0 °C,
Time 605000 sec
extruded tapes, 1N Oxalic acid; IEC 60811-404
Penetration 8.0
@Temperature 140 °C,
Time 14400 sec
[%] Hot pressure test, extruded tapes; IEC 60811-508
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 6.60e+11 ohm-cm
@Temperature 90.0 °C
500V; DIN IEC 60093
 3.50e+14 ohm-cm
@Temperature 23.0 °C
500V; DIN IEC 60093
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 125 °C
Minimum Service Temperature, Air -40.0 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 190 - 200 °CMaximum mass temperature
 190 - 210 °CTool
Zone 1 140 - 160 °C
Zone 2 150 - 170 °C
Zone 3 170 - 190 °C
Zone 4 175 - 195 °C
Zone 5 180 - 200 °C
Adapter Temperature 180 - 200 °C
Head Temperature 180 - 200 °C
Drying Temperature 60.0 - 70.0 °C
Dry Time 4.00 - 6.00 hour
Shelf Life 12.0 Month
 
Component Elements PropertiesOriginal ValueComments
Loss on Ignition(%) 30 %pressed plaques; ASTM D 2863 A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMELOS021 / 296128

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.