MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Gouda Refractories Pinnacle PP 5120H PP Random Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Product Description: 20 melt flow, random copolymer for injection molding. Pinnacle Polymers Polypropylene 5120H is made via UNIPOL™ PP technology, which utilizes gas-phase fluidized bed reactors with a high activity catalyst systems to ensure uniform physical properties and lot-to-lot consistency. This product is intended for caps, closures, and general purpose injection molding applications. This product contains a nucleation and antistatic additive package.
Features: Improved FDA food contact status; Superior color and processing stability; Low odor; Good flow and set-up behavior; Antistatic properties; Excellent lot-to-lot consistency
Pinnacle’s 5120H as marketed by Pinnacle Polymers Company, in natural, uncolored pellet form is cleared by way of FCN 1538 for use in single-and repeated-use articles intended to contact all types of food under the FDA Conditions of Use A-H. FDA has not evaluated the use of this product in contact with infant formula or breast milk.

Availability: Europe; North America

Additive: Antistatic; Nucleating Agent

Features: Antistatic; Food Contact Acceptable; Good Color Stability; Good Flow; Good Processing Stability; Low Odor; Nucleated; Random Copolymer

Uses: Caps; Closures; General Purpose

Agency Ratings: FDA FCN 1538; FDA Food Contact A-H

Appearance: Natural Color

Form: Pellets

Processing Method: Injection Molding

Information provided by Pinnacle Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.900 g/ccASTM D1505
Melt Flow 20 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 3700 psi
@Thickness 3.20 mm
Injection Molded, Type I, 2.0 in/min; ASTM D638
Elongation at Break 12 %
@Temperature -17.7 °C
Injection Molded, Type I, 2.0 in/min; ASTM D638
Flexural Modulus 137000 psi
@Thickness 3.20 mm
1% Secant, Injection Molded, Type I, 0.05 in/min; ASTM D790A
Izod Impact, Notched 0.990 ft-lb/in
@Thickness 3.20 mm
Injection Molded, Type I; ASTM D256
 2.47 ft-lb/in
@Thickness 3.20 mm
(Area) Injection Molded, Type I; ASTM D256

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPINNA814 / 311507

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.