MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Envalior Pocan® B 3215 Z 000000 PBT, 10% Glass Fiber
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

Material Notes: PBT, 10% glass fibers, injection molding, impact modified

Former Lanxess product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.36 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0011 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0011 cm/cmISO 294-4, 2577
Melt Flow 34 g/10 min
@Load 2.16 kg,
Temperature 260 °C
Estimated using room temperature density; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 85.0 MPaISO 527-1/-2
Elongation at Break 4.0 %ISO 527-1/-2
Tensile Modulus 4500 MPaISO 527-1/-2
Charpy Impact Unnotched 25.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 45.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+16 ohmIEC 60093
Dielectric Constant 3.6
@Frequency 1e+6 Hz
IEC 60250
 3.8
@Frequency 100 Hz
IEC 60250
Dielectric Strength 30.0 kV/mmIEC 60243-1
Dissipation Factor 0.0025
@Frequency 100 Hz
IEC 60250
 0.0218
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 400 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CISO 11359-1/-2
Melting Point 225 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 185 °CISO 75-1/-2
Flammability, UL94 HB
@Thickness 0.800 mm
IEC 60695-11-10
 HB
@Thickness 1.60 mm
IEC 60695-11-10
 
Processing PropertiesOriginal ValueComments
Melt Temperature 260 °CInjection Molding; ISO 294
Mold Temperature 80.0 °CInjection Molding; ISO 10724
 
Descriptive Properties
AdditivesRelease agent
FeaturesHigh impact or high impact modified
FormPellets
ISO Short NameISO 7792-1-PBT,GHPMR,09-040,GF10
ProcessingInjection molding
RegionAsia Pacific
 Europe
 Near East/Africa
 North America
 South and Central America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsubishi Rayon Acrypet® VH-001 Heat Stabilized PMMA
Envalior Pocan® B 3215 901510 PBT, 10% Glass Fiber
Envalior Pocan® BF 4130 XF 000000 PBT, 30% Glass Fiber
Envalior Pocan® KU 2-7018 000000 PBT
Envalior Pocan® BFN 4211 000000 PBT, 13% Glass Fiber Reinforced

PLANX0853 / 99068

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.