MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil Exceed™ 1018MA Film Grade Hexene LLDPE
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Hexene, Film Grade

Material Notes: Exceed™ performance PE polymers Used to formulate a wide range of film structures offering superior mechanical performance for highly demanding end-use applications.  Exceed 1018MA is an ethylene 1-hexene copolymer.  Films made from 1018MA have outstanding tensile, impact strength, and puncture.  These superior strength properties, along with excellent drawability, makes this a very versatile packaging film resin.   TnPP is not intentionally added to Exceed 1018MA. 

Availability: Africa & Middle East, Europe, North America, Asia Pacific, Latin America. 

Additive:  Exceed 1018MA: antiblock: no, slip: 1no; processing aid: yes; thermal stabilizer: yes.

Applications:  agricultural film, food packaging, multilayer packaging film, bag in box, form fill and seal packaging, over wrap film, barrier food packaging, freezer film, packaging films, blown film, general packaging, premium trash bags, blown stretch film, heavy duty bags, stand up pouches, bread bags, lamination film, trash bags.

Information provided by ExxonMobil.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.918 g/ccASTM D1505
Melt Flow 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 1400 psiASTM D882
Film Tensile Strength at Yield, TD 1400 psiASTM D882
Film Elongation at Break, MD 480 %ASTM D882
Film Elongation at Break, TD 640 %ASTM D882
Puncture Energy 35.0 in-lbExxonMobil Method
Elmendorf Tear Strength MD 250 gASTM D1922
Elmendorf Tear Strength TD 430 gASTM D1922
Dart Drop Test 590 gASTM D1709A
Film Tensile Strength at Break, MD 8500 psiASTM D882
Film Tensile Strength at Break, TD 7700 psiASTM D882
1% Secant Modulus, MD 27000 psiASTM D882
1% Secant Modulus, TD 29000 psiASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 245 °FPeak; ExxonMobil Method
 
Optical PropertiesOriginal ValueComments
Haze 29 %ASTM D1003
Gloss 28 %@ 45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEX98830 / 238214

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.