System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
3M Dyneon™ TF 4103 PTFE 15% Glass Fiber Filled
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Fluoropolymer
;
Polytetrafluoroethylene (PTFE)
;
Polytetrafluoroethylene (PTFE), Glass Filled, Molded
Material Notes:
Type II PTFE. Applications include valve seats, bearings, seals/gaskets, moldings, piston rings.
Data provided by Dyneon.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
2.21
g/cc
ASTM D4894
Apparent Bulk Density
0.820
g/cc
ASTM D4894
Particle Size
800
µm
ASTM D4894
Deformation
4.0 %
@Pressure 15.00 MPa
ASTM D621
6.0 %
@Time 86400 sec,
Pressure 15.00 MPa
ASTM D621
Mechanical Properties
Original Value
Comments
Hardness, Shore D
62
Initial; ASTM D2240
57
@Time 15.0 sec
ASTM D2240
Tensile Strength at Break
20.7
MPa
ASTM D4894
Elongation at Break
375 %
ASTM D4894
Tensile Modulus
14000
psi
ASTM D638
Thermal Properties
Original Value
Comments
CTE, linear
57.0
µm/m-°C
@Temperature 30.0 - 100 °C
ASTM E831
77.0
µm/m-°C
@Temperature 100 - 200 °C
ASTM E831
95.0
µm/m-°C
@Temperature 200 - 300 °C
ASTM E831
Thermal Conductivity
0.260
W/m-K
@Temperature 100 °C
ASTM E1530
0.270
W/m-K
@Temperature 250 °C
ASTM E1530
Shrinkage
2.2 %
ASTM D4894
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Daikin POLYFLON MG-1030 PTFE 15% Glass Fiber Filled Molding Powder
3M Dyneon™ CC603 PTFE, 15% Fiberglass Filled
PDYM80 / 34683
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.