MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Trinseo EMERGE™ 7570 Polycarbonate (PC) / Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: EMERGE™ PC/ABS 7570 advanced resin is a high flow, ignition-resistant PC/ABS blend that contains no chlorinated for brominated additives. Its superior processing makes it ideal for injection molding of large, thin-wall, or intricate parts. EMERGE™ PC/ABS 7570 is suitable for use in a wide variety of applications in the Information Technology Equipment & Consumer Electronics industries.

Applications:

  • LCD TV Enclosures
  • CRT TV Enclosures
  • Monitor and PC Enclosures

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.18 g/ccISO 1183/B
Apparent Bulk Density 0.670 g/ccISO 60
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 in/inISO 294-4
Melt Flow 20 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ISO 1133
 95 g/10 min
@Load 5.00 kg,
Temperature 260 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 47.0 MPa
@Thickness 4.00 mm
Injection Molded; ISO 527-2/50
Tensile Strength, Yield 60.0 MPa
@Thickness 4.00 mm
Injection Molded; ISO 527-2/50
Elongation at Break 40 %
@Thickness 4.00 mm
Injection Molded; ISO 527-2/50
Elongation at Yield 4.0 %
@Thickness 4.00 mm
Injection Molded; ISO 527-2/50
Tensile Modulus 2600 MPa
@Thickness 4.00 mm
Injection Molded; ISO 527-2/1
Flexural Strength 92.0 MPa
@Thickness 4.00 mm
Injection Molded, 2.0 mm/min; ISO 178
Flexural Modulus 2700 MPaInjection Molded, 2.0 mm/min; ISO 178
Izod Impact, Notched (ISO) 12.0 kJ/m²ISO 180/A
Charpy Impact, Notched 18.0 kJ/m²ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Hot Ball Pressure Test 95.0 °CIEC 60335-1
Deflection Temperature at 0.46 MPa (66 psi) 90.0 °CUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °CUnannealed; ISO 75-2/A
Vicat Softening Point 98.0 °CISO 306/B50
 105 °CISO 306/A120
Flammability, UL94 V-0
@Thickness 1.60 mm
All Colors
 V-0
@Thickness 2.50 mm
Natural plus Color
Glow Wire Ignition Temperature 800 °C
@Thickness 2.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 2.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 - 280 °C
Mold Temperature 40.0 - 80.0 °C
Drying Temperature 80.0 - 90.0 °C
Dry Time 3.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LG Chemical AF342F ABS, Flame Retardant, High Flow
Mitsubishi Xantar® C CF 407 Polycarbonate/ABS Blend
LG Chemical LUPOY GP5008BFH PC/ABS, Flame Retardance
Trinseo EMERGE™ 7560 Polycarbonate (PC) / Acrylonitrile Butadiene Styrene (ABS)
Covestro Bayblend® FR3000 PC/ABS Blend

PDWST058 / 142267

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.