MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Total 8453 Polypropylene, Random Copolymer Extrusion Grade  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polypropylene (PP); Polypropylene, Extrusion Grade

Material Notes: Random copolymer extrusion grade

Clarity/Impact - the random copolymer structure of FINA 8453 improves its clarity and impact resistance over conventional homopolymer films.

Heat Sealable - The reduced melting point of FINA 8453 makes it suitable as a heat seal layer for oriented films.

FDA - FINA 8453 complies with all applicable FDA regulations for food contact applications.

Recommended Applications - FINA 8453 is a medium ethylene content propylene copolymer product appropriate for use in a variety of applications that require improved clarity, applications that require improved clarity, flexibility, and impact strength properties or as a heat seal layer in co-extruded oriented films.

Data provided by the manufacturer, Total Petrochemicals.

Total Petrochemicals includes former Fina and Atofina plastics product lines.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.895 g/ccASTM D1505
Water Vapor Transmission 14.0 g/m²/day
@Temperature 37.8 °C
90% RH; thickness not specified; ASTM E96
Melt Flow 5.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 540 %Non-oriented film; ASTM D882
Secant Modulus 0.483 GPa1% Secant Modulus; Non-oriented Film; ASTM D882
Seal Strength >= 200 g/25 mmat 135°C, 15 psi pressure and 1 sec.
Film Tensile Strength at Break, MD 20.7 MPaNon-oriented film; ASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 134 °CDSC
 
Optical PropertiesOriginal ValueComments
Haze 2.0 %Non-oriented film; ASTM D1003
Gloss 80 %45°; Non-oriented film; ASTM D2457
 
Processing PropertiesOriginal ValueComments
Processing Temperature 120 °CHeat seal temperature.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PFIN47 / 38377

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.