MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Celanese FORTRON 1140L4 PPS, 40% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 40% Glass Fiber Filler

Material Notes: Fortron 1140L4 is a 40% glass-reinforced grade that is the strongest and toughest product available. It exhibits excellent heat and chemical resistance, good electrical properties and is inherently flame-retardant. The high hardness and rigidity at elevated temperatures allows for good load bearing performance. This product has good weldability due to the modest filler level. Applications made of this grade are electronical components (i.e. bobbins, lamp housings, brush holders) and various other components requiring strength and resistance to aggressive chemicals (i.e. automotive heaters, pumps, valves, fuel rails, microwave oven rings and distillartion column packings).

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.60 g/ccASTM D792
Density 1.64 g/ccASTM D792
 1.65 g/ccISO 1183
Water Absorption 0.020 %
@Temperature 22.8 °C
24hr immersion; ASTM D570
Water Absorption at Saturation 0.020 %ISO 62
Linear Mold Shrinkage, Flow 0.0020 - 0.0030 cm/cmASTM D955
 0.0020 - 0.0060 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0040 - 0.0060 cm/cmISO 294-4
 0.0050 - 0.0070 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 100ISO 2039-2
 100ASTM D785
Tensile Strength at Break 195 MPa5mm/min; ISO 527-2/1A
 29000 psiASTM D638
Elongation at Break 1.7 %ASTM D638
 1.9 %5mm/min; ISO 527-2/1A
Tensile Modulus 14700 MPa50mm/min; ISO 527-2/1A
 470000 psi
@Temperature 200 °C
ASTM D638
 620000 psi
@Temperature 150 °C
ASTM D638
 1.73e+6 psi
@Temperature 75.0 °C
ASTM D638
 2.10e+6 psi
@Temperature -40.0 °C
ASTM D638
Flexural Strength 285 MPaISO 178
 35000 psiASTM D790
Flexural Modulus 14500 MPaISO 178
 1.90e+6 psiASTM D790
Izod Impact, Notched 1.60 ft-lb/inASTM D256
Izod Impact, Unnotched 11.0 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
 34.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1U
Charpy Impact Unnotched 53.0 kJ/m²ISO 179/1eU
 53.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 10.0 kJ/m²ISO 179/1eA
 10.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
 1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.5
@Frequency 1000 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
ASTM D150
 4.6
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 28.0 kV/mmIEC 60243-1
Dissipation Factor 0.0010
@Frequency 1000 Hz
ASTM D150
 0.0010
@Frequency 1e+6 Hz
ASTM D150
 0.0062
@Frequency 1e+6 Hz
IEC 60250
Arc Resistance 134 secASTM D495
Comparative Tracking Index 125 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 26.0 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 42.0 µm/m-°CISO 11359-2
Specific Heat Capacity 1.50 J/g-°C
Melting Point 280 °C10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 536 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 270 °CISO 75-1, -2
 509 °FASTM D648
Deflection Temperature at 8.0 MPa 215 °CISO 75-1, -2
Glass Transition Temp, Tg 90.0 °CISO 11357-1,-2,-3
Flammability, UL94 V-0
@Thickness 1.50 mm
 5VA
@Thickness 3.00 mm
Oxygen Index 47 %ISO 4589
 
Processing PropertiesOriginal ValueComments
Processing Temperature 140 - 160 °Ccavity
 330 - 340 °Chot runner
Feed Temperature 60.0 - 80.0 °C
Zone 1 290 - 300 °C
Zone 2 310 - 320 °C
Zone 3 330 - 340 °C
Zone 4 330 - 340 °C
Die Temperature 310 - 330 °C
Melt Temperature 310 - 340 °CISO 294
 330 - 340 °C
Mold Temperature 135 - 160 °CISO 294
Drying Temperature 130 - 140 °C
Dry Time 3.00 - 4.00 hour
Moisture Content <= 0.020 %
Injection Pressure 50.0 - 100 MPa
Hold Pressure 30.0 - 70.0 MPa
Back Pressure <= 3.00 MPa
Screw Speed 50 rpm
@Diameter 55.0 mm
 75 rpm
@Diameter 40.0 mm
 120 rpm
@Diameter 25.0 mm
 
Descriptive Properties
Injection moldingYes
Injection speedfast

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese FORTRON 1140L6 PPS, 40% Glass Reinforced
Celanese FORTRON 1140L0 PPS, 40% Glass Reinforced
Celanese FORTRON 1140L4-T PPS, Glass Reinforced
Celanese FORTRON 1141L4 PPS, 40% Glass Reinforced
Celanese FORTRON 11400000000 PPS, 40% Glass Reinforced

PHCQ271 / 178726

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.