MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Copper Alloy, UNS C18100, H04 Temper, Wire
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Hard

Fabrication Properties: Excellent Suitability – Soldering, Capacity for Being Cold Worked, Capacity for Being Hot Formed; Good Suitability – Brazing, Gas Shielded Arc Welding; Fair Suitability – Butt Weld

Common Fabrication Processes: Bending, Drawing, Extruding, Heading, Hot forging, Hot rolling, Machining, Swaging

Typical Uses: Circuit Breakers; Contacts; Heat Sinks; High Temperature Wire; Resistance Welding Tips; Resistance Welding Wheels; Semi Conductor Bases; Switches; Continuous Casting Molds; Fasteners; Fusion Energy Targets; Resistance Welding Equipment; Solar Collectors; Stressed Parts

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.319 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 80
@Thickness 233 mm
Tensile Strength 70.0 ksi
@Thickness 4.06 mm
 70.0 ksi
@Thickness 1.02 mm
 72.0 ksi
@Thickness 20.3 mm
 73.0 ksi
@Thickness 20.3 mm
 75.0 ksi
@Thickness 233 mm
 80.0 ksi
@Thickness 20.3 mm
 85.0 ksi
@Thickness 20.3 mm
Tensile Strength, Yield 63.0 ksi
@Thickness 4.06 mm
 66.0 ksi
@Thickness 20.3 mm
 66.0 ksi
@Thickness 20.3 mm
 68.0 ksi
@Thickness 233 mm
 69.0 ksi
@Thickness 20.3 mm
 75.0 ksi
@Thickness 20.3 mm
Elongation at Break 4.0 %
@Thickness 20.3 mm
 5.0 %
@Thickness 20.3 mm
 6.0 %
@Thickness 4.06 mm
 10 %
@Thickness 1.02 mm
 11 %
@Thickness 233 mm
 12 %
@Thickness 20.3 mm
 13 %
@Thickness 20.3 mm
Tensile Modulus 18200 ksi
Modulus of Rigidity 6800 ksi
Poissons Ratio 0.34Calculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000220 ohm-cm80% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.30 µin/in-°F
@Temperature 20.0 - 100 °C
 10.2 µin/in-°F
@Temperature 20.0 - 200 °C
 10.7 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0940 BTU/lb-°F
Thermal Conductivity 187 BTU-in/hr-ft²-°F
Melting Point <= 1967 °F
Liquidus 1967 °F
Annealing Point 1100 - 1300 °F
 
Processing PropertiesOriginal ValueComments
Solution Temperature 1650 - 1790 °F
@Time 60.0 sec
Water
Hot-Working Temperature 1450 - 1700 °F
Precipitation Temperature >= 840 °FAir
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr 0.40 - 1.2 %
Copper, Cu >= 98.7 %
Magnesium, Mg 0.030 - 0.060 %
Zirconium, Zr 0.080 - 0.20 %
 
Descriptive Properties
Cold Work (%)600.16 in
 609.16 in
 750.8 in
 750.8 in
 900.8 in
 900.8 in
 990.04 in

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC18100x2 / 291625

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.