MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Cabot CABELEC® CA4676 LDPE, Conductive Compound
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: Product highlights: CABELEC CA4676 electrically conductive compound is based on conductive carbon black dispersed in a modified low density polyethylene resin. Its electrical and mechanical properties are permanent and are not dependent on atmospheric conditions.

Key applications: CABELEC CA4676 conductive compound has been specially designed for packaging and product handling applications where freedom from the hazard of electrostatic discharge is necessary. Examples of use are in handling of explosive powders, pigments and electronic components and it is particularly suitable for foam applications.

Information provided by Cabot Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.990 g/ccISO 1183
Melt Flow 1.0 g/10 min
@Load 190 kg,
Temperature 5.00 °C
ISO 1133
 5.0 g/10 min
@Load 190 kg,
Temperature 10.0 °C
ISO 1133
 28 g/10 min
@Load 190 kg,
Temperature 21.6 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 13.0 MPa3 mm compressed plaque; ISO 527
Tensile Strength, Yield 11.0 MPa3 mm compressed plaque; ISO 527
Elongation at Break 385 %3 mm compressed plaque; ISO 527
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity <= 10 ohm-cm4 mm compressed plaque; IEC62631-3-1
Surface Resistance <= 10000 ohm100 µm film; IEC62631-3-2
 
Processing PropertiesOriginal ValueComments
Processing Temperature 120 - 160 °CExtrusion
Drying Temperature 80.0 °C
Dry Time 2.00 - 4.00 hour
 
Descriptive Properties
Product FormPellets

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCABOT042 / 315777

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.