MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
ECO Brass, Copper Alloy, UNS C69300, H02 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Temper: 1/2 Hard

Fabrication Properties: Excellent Suitability – Soldering, Capacity for Being Hot Formed; Good Suitability – Brazing, Oxyacetylene Welding, Gas Shielded Arc Welding, Coated Metal Arc Welding, Spot Weld, Seam Weld, Butt Weld; Poor Suitability – Capacity for Being Cold Worked

Common Fabrication Processes: Forming and Bending; Machining; Shearing

Typical uses: Fluid Connectors; Sensor Bodies; Thermostat Parts; Automatic Screw Machine Parts; Bolts; Condenser Tube Plate; Nuts; Pneumatic Fittings; Pump Parts; Screw Machine Products; Valve Bodies for Water; Valve Stems; Marine Products; Propeller Shafts; Faucet Stems; Faucets; Plumbing Fittings; Water Meter Cases

Applicable Specifications: Die Forging – ASTM B283/B283M; Rod – ASTM B371/B371M; Rod, Bar & Shapes – Forgings ASTM B124/B124M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.300 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 80
@Thickness 50.8 mm
 85
@Thickness 38.1 mm
 >= 90
@Thickness 25.4 mm
 95
@Thickness 6.35 mm
 97
@Thickness 12.7 mm
Tensile Strength 80.0 ksi
@Thickness 50.8 mm
 87.0 ksi
@Thickness 38.1 mm
 88.0 ksi
@Thickness 25.4 mm
 103 ksi
@Thickness 2.54 mm
 105 ksi
@Thickness 12.7 mm
 114 ksi
@Thickness 6.35 mm
Tensile Strength, Yield 48.0 ksi
@Thickness 50.8 mm
0.2% Offset
 49.0 ksi
@Thickness 25.4 mm
0.2% Offset
 49.0 ksi
@Thickness 38.1 mm
0.2% Offset
 49.0 ksi
@Thickness 50.8 mm
0.5% Ext
 50.0 ksi
@Thickness 25.4 mm
0.5% Ext
 50.0 ksi
@Thickness 38.1 mm
0.5% Ext
 60.0 ksi
@Thickness 12.7 mm
0.5% Ext
 61.0 ksi
@Thickness 6.35 mm
0.5% Ext
 73.0 ksi
@Thickness 12.7 mm
0.2% Offset
 74.0 ksi
@Thickness 6.35 mm
0.2% Offset
Elongation at Break >= 5.0 %
@Thickness 2.54 mm
 >= 5.0 %
@Thickness 6.35 mm
 >= 5.0 %
@Thickness 12.7 mm
 >= 10 %
@Thickness 38.1 mm
 >= 10 %
@Thickness 50.8 mm
 10 %
@Thickness 25.4 mm
Tensile Modulus 15200 ksi
Fatigue Strength 23000 psi
@Thickness 25.4 mm,
# of Cycles 1.00e+8
Machinability 85 %
Forgeability 95 %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000220 ohm-cm8% IACS
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.3 µin/in-°F
@Temperature 20.0 - 100 °C
 10.3 µin/in-°F
@Temperature 20.0 - 200 °C
 10.4 µin/in-°F
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.0900 BTU/lb-°F
Thermal Conductivity 21.8 BTU-in/hr-ft²-°F
Melting Point 1571 - 1616 °F
Solidus 1571 °F
Liquidus 1616 °F
Annealing Point 932 - 1112 °F
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 73 - 77 %
Iron, Fe <= 0.10 %
Lead, Pb <= 0.090 %
Manganese, Mn <= 0.10 %
Nickel, Ni <= 0.10 %
Phosphorus, P 0.040 - 0.15 %
Silicon, Si 2.7 - 3.4 %
Tin, Sn <= 0.20 %
Zinc, Zn 19 - 24.3 %As Balance
 
Descriptive Properties
Cold Work (%)130.5 in
 150.10 in
 22.0 in
 41.5 in
 51.0 in
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC69300x4 / 292375

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.